Embodiment 1
[0033] Mix 20 parts of ethylene-acrylic acid copolymer, 15 parts of polyurethane resin and 61.4 parts of soft water, start heating and stirring, stir at 100r / min, 70°C and add 1 part of polycarbodiimide and 0.1 part of N-hydroxysuccinide Amine, continue to stir for 5 minutes, the temperature drops to 45 ° C, add 2 parts of heat-activated adhesive and continue to stir for 20 minutes, after cooling down to normal temperature, add 0.5 parts of nonionic antistatic agent under stirring to obtain a water-based coating solution. The water-based coating solution is used A 120-mesh anilox roller is coated on a medical wristband, and the sample is obtained after printing by HP Indigo. The printed appearance is good, the color is uniform, and the color difference is 0.45△E. The printed wristband is soaked in soft water and left for 7 days. It is whitish and has a good appearance.
Embodiment 2
[0035] Mix 25 parts of ethylene-acrylic acid copolymer, 20 parts of polyurethane resin and 47.6 parts of soft water, start heating and stirring, stir at 100r / min, 70°C and add 2 parts of polycarbodiimide and 0.4 parts of N-hydroxysuccinide Amine, continue to stir for 5 minutes, the temperature drops to 45 ° C, add 4 parts of heat-activated adhesive and continue to stir for 20 minutes, after cooling down to normal temperature, add 1 part of non-ionic antistatic agent under stirring to obtain a water-based coating solution. The water-based coating solution is used A 120-mesh anilox roller is coated on a medical wristband, and the sample is obtained after printing by HPIndigo. The printed appearance is good, the color is uniform, and the color difference is 0.37△E. White, good appearance.
Embodiment 3
[0037] Mix 30 parts of ethylene-acrylic acid copolymer, 30 parts of polyurethane resin and 29 parts of soft water, start heating and stirring, stir at 100r / min, 70°C and add 3 parts of polycarbodiimide and 1 part of N-hydroxysuccinimide Amine, continue to stir for 5 minutes, the temperature drops to 45 ° C, add 5 parts of heat-activated adhesive and continue to stir for 20 minutes, after cooling down to normal temperature, add 2 parts of non-ionic antistatic agent under stirring to obtain a water-based coating solution. The water-based coating solution is used A 120-mesh anilox roller is coated on a medical wristband, and the sample is obtained after printing by HP Indigo. The printed appearance is good, the color is uniform, and the color difference is 0.40△E. The printed wristband is soaked in soft water and left for 14 days. It is whitish and has a good appearance.