A kind of semi-worsted dream color yarn and its preparation method
A semi-worsted, dream-colored technology, applied in the field of yarn, can solve the problems of limited use and high price, and achieve the effects of reducing static electricity, good elasticity and reducing noil rate.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] Taking colored polyester fiber, colored viscose fiber and wool fiber 18.3 tex semi-worsted dream color blended yarn as an example, the weight percentage of the blended color polyester fiber, colored viscose fiber and wool fiber is 40:40:20.
[0031] Its preparation method is as follows:
[0032] (1) Raw material and wool process: add antistatic agent accounting for 1.5% of the weight of the raw material, mix and open the raw material twice or three times when mixing the wool; the reconciled raw material is stored in the wool warehouse between the wool and wool for 24- 48 hours;
[0033] (2) Carding and sliver making process: the relative humidity of the workshop environment is controlled above 80%, the sliver weight is 16.9g / 5m, the sliver speed is 39.2m / min, the wool feeding amount is 42g / time, and the licker-in speed is 630~760r / min , the cylinder speed is 330~375r / min, and the distance between the cylinder and the cover is 12, 10, 10, 10, 12 / 1000 inches;
[0034] (...
Embodiment 2
[0040] Taking colored polyester fiber, colored viscose fiber and wool fiber 27.8 tex semi-worsted dream color blended yarn as an example, the weight percentage of the blended color polyester fiber, colored viscose fiber and wool fiber is 50:35:15.
[0041] Its preparation method is as follows:
[0042] (1) Raw material and wool process: add antistatic agent accounting for 1.5% of the weight of the raw material, mix and open the raw material twice when mixing the wool; the reconciled raw material is stored in the hair warehouse between the wool and wool for 24 hours;
[0043] (2) Carding and sliver making process: the relative humidity of the workshop environment is controlled above 80%, the sliver weight is 16.9g / 5m, the sliver speed is 39.2m / min, the wool feeding amount is 42g / time, the licker-in roller speed is 630r / min, tin Lining speed 330~375r / min, cylinder to cover plate gauge is 12, 10, 10, 10, 12 / 1000 inches;
[0044] (3) Drawing process: the temperature of the worksh...
Embodiment 3
[0050] Taking colored polyester fiber, colored viscose fiber and wool fiber 28.3 tex semi-worsted dream color blended yarn as an example, the weight percentage of colored polyester fiber, colored viscose fiber and wool fiber blended is 55:20:25.
[0051] Its preparation method is as follows:
[0052] (1) Raw material and wool process: add antistatic agent accounting for 1.5% of the weight of the raw material, mix and open the raw material twice or three times when mixing the wool; the reconciled raw material is stored in the wool warehouse between the wool and wool for 24- 48 hours;
[0053] (2) Carding and sliver making process: the relative humidity of the workshop environment is controlled above 80%, the sliver weight is 16.9g / 5m, the sliver speed is 39.2m / min, the wool feeding amount is 42g / time, the licker-in roller speed is 760r / min, tin Lining speed 330~375r / min, cylinder to cover plate gauge is 12, 10, 10, 10, 12 / 1000 inches;
[0054](3) Drawing process: the temperat...
PUM
Property | Measurement | Unit |
---|---|---|
length | aaaaa | aaaaa |
length | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com