Embodiment 1
[0022] The cashmere sanding treatment method comprises the steps of:
[0023] ①, pretreatment
[0024] Add cashmere and formic acid of 0.25% cashmere weight to the drum (the raw materials involved in the following are all commercial grades), and adjust the pH value to 3.5, and rotate for 1.5h;
[0025] Add 0.55% cashmere weight degreaser to the drum, and rotate for 0.5h;
[0026] Add 1.5% cashmere weight HN solution to the drum, and rotate for 2.5 hours for retanning;
[0027] ②, dyeing treatment
[0028] Add the retanning agent magnopal DP of 30% cashmere weight in the drum, and rotate for 0.5h;
[0029] Add sodium formate of 1% cashmere weight to the drum, and adjust the pH value to 5.6, and rotate for 1.5h;
[0030] Add cationic fatliquor with 11% cashmere weight to the rotating drum, and rotate for 1.2h;
[0031] Add cationic resin retanning agent of 1.8% cashmere weight in the rotating drum, and rotate for 5 minutes;
[0032] Add the dye solution to the drum and rot...
Embodiment 2
[0037] The cashmere sanding treatment method comprises the steps of:
[0038] ①, pretreatment
[0039] Add cashmere and formic acid of 0.2% cashmere weight to the drum, and adjust the pH value to 3.6, and rotate for 1 hour;
[0040] Add 0.6% cashmere weight degreasing agent to the drum, and rotate for 0.5h;
[0041] Add 2% cashmere weight HN solution to the drum, and rotate for 2 hours for retanning;
[0042] ②, dyeing treatment
[0043] Add the retanning agent magnopal DP of 30% cashmere weight in the drum, and rotate for 0.5h;
[0044] Add 1.5% sodium formate by weight of cashmere to the drum, adjust the pH value to 5.5, and rotate for 1.5 hours;
[0045] Add cationic fatliquor of 8% cashmere weight to the rotating drum, and rotate for 1.5h;
[0046] Add cationic resin retanning agent of 1.5% cashmere weight in the drum, and rotate for 5 minutes;
[0047] Add the dye solution to the drum and rotate for 1 min;
[0048] Add a color-fixing agent of 1% cashmere weight in ...
Embodiment 3
[0052] The cashmere sanding treatment method comprises the steps of:
[0053] ①, pretreatment
[0054] Add cashmere and formic acid of 0.3% cashmere weight to the drum, and adjust the pH value to 3.4, and rotate for 2 hours;
[0055] Add 0.5% cashmere weight degreaser to the drum, and rotate for 1 hour;
[0056] Add 1% cashmere weight HN solution to the drum, and rotate for 3 hours for retanning;
[0057] ②, dyeing treatment
[0058] Add the retanning agent magnopal DP of 25% cashmere weight in the drum, and rotate for 1h;
[0059] Add sodium formate of 1% cashmere weight to the drum, and adjust the pH value to 5.7, and rotate for 1 hour;
[0060] Add cationic fatliquor with 14% cashmere weight in the rotating drum, and rotate for 1 hour;
[0061] Add cationic resin retanning agent of 2% cashmere weight to the drum, and rotate for 1 min;
[0062] Add the dye solution to the drum and rotate for 3 minutes;
[0063] Add 0.5% color-fixing agent of cashmere weight in the rot...