Embodiment approach 1
[0013] Dissolve 0.05mol silver nitrate in 50mL distilled water to make 1mol / L silver ion aqueous solution; dissolve 0.025mol potassium pyrophosphate in 100mL distilled water to make 0.25mol / L pyrophosphate solution; slowly drop silver ions Add it into the pyrophosphate solution, stir vigorously for 10 minutes; filter the resulting precipitate with suction, wash it with distilled water and absolute ethanol in turn, and then dry it in vacuum at 60°C for 6 hours to obtain a silver pyrophosphate photocatalyst.
Embodiment approach 2
[0015] Potassium pyrophosphate in embodiment 1 is replaced by sodium tripolyphosphate, and the concentration of tripolyphosphate is 0.33mol / L.
Embodiment approach 3
[0017] The potassium pyrophosphate in embodiment 1 is replaced by sodium metaphosphate, and the concentration of sodium metaphosphate is 0.16mol / L.
[0018] The photocatalyst prepared by the present invention can be supported on a carrier, and the present invention is not limited to the above embodiments.