An improved batching process for wear-resistant cast iron

A technology of wear-resistant cast iron and batching technology, which is applied in the field of mechanical material processing, can solve the problems of inability to harden, reduce the wear resistance of the working interface, and reduce the wear resistance of wear-resistant parts, so that it is not easy to be impacted and broken, and the wear resistance is enhanced. Effect of improving corrosion resistance

Active Publication Date: 2016-06-22
XIANGYANG TO WIN MACHINERY
View PDF3 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] (1) The as-cast carbides are distributed in a network shape and are easy to break when subjected to impact loads, and will peel off in pieces in actual use;
[0004] (2) After quenching at 1050°C + tempering at 180°C, there is a chromium troostite matrix structure, austenite content is very small, the toughness is not high enough, and it cannot be hardened when impacted, reducing the wear resistance of the working interface
[0005] Usually wear-resistant cast iron structure such as figure 1 As shown, these shortcomings greatly reduce the wear resistance of wear parts. For example, the service life of wear-resistant pipes for conveying cement is only 40,000 cubic meters per piece

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • An improved batching process for wear-resistant cast iron
  • An improved batching process for wear-resistant cast iron

Examples

Experimental program
Comparison scheme
Effect test

Embodiment Construction

[0018] Select the following ingredients (calculated by mass percentage), and the total weight is calculated by 1000 kg:

[0019] Carbon: 3.3%; Silicon: 0.6%; Manganese: 1.4%; Chromium: 25%; Nickel: 1.1%; Molybdenum: 1.3%; Vanadium: 0.8%; Sulfur: 0.03%;

[0020] The process steps for forming wear-resistant cast iron are as follows:

[0021] (1) 23.6 kg of ferromolybdenum containing 55% molybdenum and 1.5% silicon (containing 1.3% molybdenum and 0.04% silicon after conversion), and 11 kg of nickel plate containing 99.9% nickel (1.1% nickel after conversion) , 417 kg of low-carbon ferrochromium containing 60% chromium, 1% silicon, and 1.5% carbon (converted to contain 25% chromium, 0.42% silicon, and 0.63% carbon), 25 kg of carbon 99.9 recarburizer (contains 2.5% carbon after conversion) and 494.4 kg of steel scrap with 0.26% carbon, 0.22% silicon, 0.40% manganese and 0.30% vanadium (0.13% carbon after conversion, silicon 0.21%, containing 0.2% manganese, containing 0.15% vanad...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
elongationaaaaaaaaaa
elongationaaaaaaaaaa
Login to View More

Abstract

The name of the invention is an improved wear-resistant cast iron batching process. It belongs to the technical field of mechanical material processing. The main purpose is to solve the shortcomings of poor wear resistance and short service life of wear-resistant cast iron. Its main features are: the components include: 3.1-3.4% carbon, 0.6-1.0% silicon, 0.8-1.4% manganese, 23-26% chromium, 1.0-1.4% nickel, 1.0-1.4% Molybdenum, 0.5-1.0% vanadium, ≤0.04% sulfur, ≤0.06% phosphorus, and the balance is iron, totaling 100%; the process steps for forming wear-resistant cast iron are as follows: (1) Add molybdenum iron and nickel plates into the medium frequency induction furnace , ferrochromium, recarburizer and scrap steel are melted; (2) add ferromanganese and ferrovanadium; (3) sulfur and phosphorus should be controlled within the above range; (4) when the temperature reaches 1500-1540 °C, pour the product; (5) the product is quenched at 1050 °C and Heat treatment with 180°C tempering. The improved wear-resistant cast iron is greatly improved in terms of wear resistance and corrosion resistance in weak acid and alkali environments, and is especially suitable for the production of concrete mixer lining plates, conveying pipeline lining pipes and other carriers in the construction process of the engineering construction industry.

Description

technical field [0001] The invention belongs to the technical field of mechanical material processing, and in particular relates to a casting and smelting process. Background technique [0002] In the engineering and construction industry, high chromium cast iron wear parts are often used, but the usual high chromium cast iron wear parts have the following shortcomings: [0003] (1) The as-cast carbides are distributed in a network shape and are easy to break when subjected to impact loads, and will peel off in pieces in actual use; [0004] (2) After quenching at 1050°C + tempering at 180°C, there is a chromium troostite matrix structure, the austenite content is very small, the toughness is not high enough, and it cannot be hardened when impacted, which reduces the wear resistance of the working interface. [0005] Usually wear-resistant cast iron structure such as figure 1 As shown, these shortcomings greatly reduce the wear resistance of wear-resistant parts, such as t...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityPatents(China)
IPC IPC(8): C22C37/10C22C33/08
Inventor张立波张爱国何凯
OwnerXIANGYANG TO WIN MACHINERY