Looking for breakthrough ideas for innovation challenges? Try Patsnap Eureka!

A kind of glaze for ultra-thin ceramic rock plate and its preparation method and application

A technology for ceramics and slabs, which is applied in the field of glazes for ultra-thin ceramic slabs and its preparation. It can solve the problems of limited glaze application, easy-to-crack products, and high prices, so as to improve the hiding power and color development performance, and improve the fracture mode. Number, the effect of improving stability

Active Publication Date: 2022-02-01
FOSHAN SANSHUI CREATE TIDE
View PDF0 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, the glaze used in the traditional bell jar glazing and spraying process is pure water glaze, and water easily penetrates the green body and seriously affects the strength of the green body of this type of rock slab products, resulting in easy cracking during the firing process or products in the later stage. It is easy to break during processing, so it is not suitable for glazing of this kind of slate products
However, the digital spray glazing process of digital glaze requires an expensive inkjet printer and nozzle, and compared with the traditional glazing process, the amount of glaze applied by the digital spray glazing process is limited, resulting in limited hiding power of the digital glaze, resulting in ultra-thin ceramic rock slabs The color of the product is poor, the wear resistance is poor, and the glaze is not fine enough, which leads to the poor texture of the ultra-thin ceramic rock plate product

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0072] A preparation method of a glaze for ultra-thin ceramic rock slabs of the present embodiment comprises the following steps:

[0073] Preparation of step S1 top glaze:

[0074] Step S11, add 13% ethylene glycol, 10% glycerin, 0.1% Surfynol 440, 0.1% Tego® Foamex 810, 0.3% BYK-410 and 3% self-made anhydrous polyacrylic acid dispersant into the vertical sand mill, Stir well to form a transparent solution 1.

[0075] Step S12, slowly add 20% albite, 9% dolomite, 5.5% bauxite, 5.5% zirconium silicate and 5% matte frit powder to transparent solution 1 (matte frit powder consists of 58% SiO 2 , 23% Al 2 o 3 , 5.6%K 2 O, 3.2% Na 2 O, 3% CaO, 5.2% MgO and 2% SrO), grind while stirring, the grinding medium is 1mm zirconia ball, grind to D 97 was 7.798 μm, and glaze suspension 1 was obtained.

[0076] Step S13, adding the remaining 18.5% ethylene glycol and 10% glycerin to the above glaze suspension 1 for performance adjustment, the adjusted glaze suspension 1 has a viscosi...

Embodiment 2

[0086] A preparation method of a glaze for ultra-thin ceramic rock slabs of the present embodiment comprises the following steps:

[0087] Preparation of step S1 top glaze:

[0088] Step S11, 9% ethylene glycol, 15% diethylene glycol, 0.15% Tego® Wet 505, 0.15% SN-Defoamer485, 0.5% Vok®-Keperrhevok-422 and 2.5% self-made anhydrous polyacrylic acid dispersant were added to In a vertical sand mill, stir evenly to form a transparent solution 1.

[0089] Step S12, slowly add 21% albite feldspar, 12% dolomite, 6% bauxite, 6% zirconium silicate and 3% matte frit powder to transparent solution 1 (matte frit powder consists of 63% SiO 2 , 20% Al 2 o 3 , 3%K 2 O, 4.2% Na 2 O, 4.2% CaO, 2% MgO and 3.6% SrO), grind while stirring, the grinding medium is 1mm zirconia ball, grind to D 97 was 9.237 μm, and glaze suspension 1 was obtained.

[0090] Step S13, adding the remaining 14.7% ethylene glycol and 10% diethylene glycol to the above glaze suspension 1 for performance adjustment...

Embodiment 3

[0100] A preparation method of a glaze for ultra-thin ceramic rock slabs of the present embodiment comprises the following steps:

[0101] Preparation of step S1 top glaze:

[0102] Step S11, mix 10% isopropanol, 14% glycerin, 5% diethylene glycol monobutyl ether, 0.15% Toynol® Superwet-300, 0.15% Tego® Foamex 810, 0.5% Vok®-Keperrhevok-422 and 3% Add the self-made anhydrous polyacrylic acid dispersant into a vertical sand mill, and stir evenly to form a transparent solution 1.

[0103] Step S12, slowly add 23% albite feldspar, 12% dolomite, 6% bauxite, 6% zirconium silicate and 5% matte frit powder to transparent solution 1 (matte frit powder consists of 62% SiO 2 , 21% Al 2 o 3 , 3%K 2 O, 3% Na 2 O, 4% CaO, 4% MgO and 3% SrO), grind while stirring, the grinding medium is 1mm zirconia ball, grind to D 97 was 7.337 μm, and glaze suspension 1 was obtained.

[0104] Step S13, adding the remaining 5.2% glycerin and 10% diethylene glycol monobutyl ether to the above-mentio...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to a glaze for ultra-thin ceramic rock slabs, a preparation method and application thereof. The glaze includes surface glaze and protective glaze. The surface glaze is composed of specific content of surface glaze dry material, water-soluble organic solvent, wetting and leveling agent, defoamer, anti-settling agent and dispersant; surface glaze dry material is composed of specific content Albite, dolomite, high alumina bauxite, zirconium silicate and matte frit powder; the protective glaze is composed of a specific content of protective glaze dry material, water-soluble organic solvent, wetting and leveling agent, defoamer, It is composed of anti-settling agent and dispersant; the protective glaze dry material is composed of specific content of wollastonite, albite, kaolin, burnt talc, calcined zinc oxide, calcined alumina and bright frit powder; the dispersant is self-made anhydrous poly Acrylic dispersant. The glaze is suitable for the high-pressure spray glaze process, and after being sprayed on the surface of the ultra-thin ceramic rock slab with a thickness of 3mm or less by the high-pressure spray process, it will not affect the strength of the body, effectively reducing the defect rate of the product after firing, and Low glazing cost and high product quality.

Description

technical field [0001] The invention relates to the technical field of glazes, in particular to a glaze for ultra-thin ceramic rock slabs and a preparation method and application thereof. Background technique [0002] In recent years, ceramic rock slabs are widely used as home decoration materials because they can withstand cutting, drilling, grinding and other processing processes. They can be used for background walls, cabinets, wardrobes, tea sets, bathroom cabinets, sinks, doors and Kitchen cooktop panels, etc. The rock slabs used for cabinets and wardrobes are generally required to use ultra-thin ceramic rock slabs with a thickness of 3mm, and the production of 3mm ultra-thin ceramic rock slabs is still a technical difficulty that needs to be overcome urgently in China. Only a few domestic companies can Most of the production is imported from Italy. The production difficulty of this kind of slate products is that the bricks are too thin and the strength is low. How to...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C03C8/20C03C8/16C03C8/02C03C8/04C04B41/89C08F283/06C08F220/06C08F212/08
CPCC03C8/20C03C8/16C03C8/02C03C8/04C04B41/89C04B41/52C08F283/065C04B41/5022C04B41/4539C04B41/4543C08F220/06C08F212/08
Inventor 周军张天杰戴建斌刘腾邓佳平肖元成王衔雯
Owner FOSHAN SANSHUI CREATE TIDE
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products