A technology for automotive interiors and artificial leather, applied in the field of artificial leather for automotive interiors and its preparation, can solve problems such as poor wear resistance and easy peeling off of the coating, so as to improve wear resistance, maintain softness and comfort, and improve experience Sensitive effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] A preparation method of artificial leather for automobile interior, comprising the following steps:
[0020] Step 1: Mix 40 parts of PVC resin, 3 parts of dibutyl phthalate, and 0.5 part of foaming agent at 50°C to obtain foam layer slurry;
[0021] Step 2: Roll the foamed layer slurry obtained above to 0.5mm on release paper, and dry at 80°C;
[0022] Step 3: Mix 80 parts of polycarbonate resin, 3 parts of curing agent, 0.1 part of defoamer, and 1 part of leveling agent at 70° C. to obtain a resin layer slurry; apply 1 mm of the resin layer slurry to The surface of the foam layer is dried at 80°C;
[0023] Step 4: Put 50 parts of PU, 1 part of leveling agent, 0.5 part of defoamer, 8 parts of cross-linking agent, 50 parts of water-based self-extinguishing polycarbonate resin, 6 parts of silicone wear-resisting aid, and 5 parts of hand feeling aid. Mixing at 100° C. for 3 hours to obtain a surface treatment agent, coating the surface treatment agent on the surface of t...
Embodiment 2
[0025] A preparation method of artificial leather for automobile interior, comprising the following steps:
[0026] Step 1: Mix 50 parts of PVC resin, 5 parts of dibutyl phthalate, and 0.8 part of foaming agent at 60°C to obtain foam layer slurry;
[0027] Step 2: Roll the foamed layer slurry obtained above to 0.8 mm on release paper, and dry;
[0028] Step 3: Mix 80 parts of polycarbonate resin, 3 parts of curing agent, 0.1 part of defoamer, and 2 parts of leveling agent at 70° C. to obtain resin layer slurry; The surface of the foam layer is dried at 80°C;
[0029] Step 4: Put 50 parts of PU, 1 part of leveling agent, 0.5 part of defoamer, 13 parts of cross-linking agent, 60 parts of polycarbon resin, 8 parts of silicone wear-resisting aid, and 6 parts of hand feeling aid at 150°C After mixing for 2 hours, a surface treatment agent was obtained, the surface treatment agent was coated on the surface of the resin layer, and the artificial leather was obtained after drying at...
Embodiment 3
[0031] A preparation method of artificial leather for automobile interior, comprising the following steps:
[0032] Step 1: uniformly mix 35 parts of PVC resin, 1 part of plasticizer and 0.5 part of foaming agent at 50°C to obtain foam layer slurry;
[0033] Step 2: Roll the foamed layer slurry obtained above to 0.5mm on release paper, and dry;
[0034] Step 3: Mix 70 parts of polycarbonate resin, 2 parts of curing agent, 0.05 part of defoamer, and 1 part of leveling agent at 60° C. to obtain a resin layer slurry; apply the resin layer slurry to 1.2 mm On the surface of the foam layer, drying;
[0035] Step 4: Put 40 parts of PU, 0.5 parts of leveling agent, 0.3 parts of defoamer, 5 parts of cross-linking agent, 50 parts of polycarbon resin, 6 parts of silicone wear-resistant additives, and 5 parts of hand feeling additives at 100°C Mixing for 1 hour to obtain a surface treatment agent, coating the surface treatment agent on the surface of the resin layer, and drying at 100°...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com