Method for preparing modified asphalt mixture using waste and old tyre and hybrid method
A technology of waste tires and modified asphalt, which is applied to building insulation materials, on-site coagulation pavement, building components, etc., to achieve the effects of prolonging service life, reducing road traffic noise, and environmental protection engineering benefits
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0034] Example 1: Preparation of rubber-modified asphalt mixture at the construction site
[0035] (1) Preparation of rubber asphalt
[0036] The base asphalt is AH-70 asphalt, and its technical indicators are shown in Table 1. The fine rubber powder is crushed and ground from waste tires at room temperature to obtain 80-mesh fine rubber powder with a relative density of 1.15.
[0037] Table 1AH-70 asphalt technical indicators
[0038]
[0039] The AH-70 asphalt is heated to 190°C, the amount of fine rubber powder is determined to be 15% of the mass of the base asphalt, and the mixing temperature is controlled at 190°C-195°C. Use a high-speed shearing device to mix for 15 minutes, and the stirring speed is 1500 rpm, so that the fine rubber powder is evenly dispersed in the base asphalt, and then continue to stir for 45 minutes, so that the fine rubber powder and the base asphalt can fully react at high temperature, reaching Desired binder properties. Table 2 is the perf...
Embodiment 2
[0057] Example 2: Preparation of rubber-modified asphalt mixture in the laboratory
[0058] The coarse aggregate that adopts in the present embodiment is basalt, and the Vita joint agent of 5% (the mass number of rubber powder) is mixed in the preparation process of rubber asphalt, all the other raw materials are identical with embodiment 1, and the adding of Vita joint agent promotes The rubber powder is chemically combined with the bitumen to reduce the precipitation of the rubber powder.
[0059] (1) Preparation of rubber asphalt
[0060] The dosage of fine rubber powder is 15% of the mass of asphalt, and the dosage of Vita coupling agent is 5% of the mass of rubber powder. The mixing temperature is controlled at 185°C-190°C. First use a high-speed shearing device to mix for 20 minutes, and the stirring speed is 3000 rpm, so that the fine rubber powder and Vita coupling agent are evenly dispersed in the base asphalt, and then continue to stir for 40 minutes to make them f...
PUM
| Property | Measurement | Unit |
|---|---|---|