A production method and glass technology, applied in the production field of non-imprinted glass, can solve the problems that the glass surface is easily stained with oil stains, fingerprints, sweat stains, destroy the chemical structure of the glass surface, affect the aesthetics of the glass, etc., and achieve a delicate and smooth hand feel. , The effect of simple procedure and stable product quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] Taking patterned jade sand glass as an example, a production method of non-printed glass, the production process steps are as follows:
[0016] (1) the jade sand glass is cleaned and dried with a cleaning machine equipped with ionized water and drying equipment;
[0017] (2) Place the cleaned jade sand glass on a screen with a designed pattern for printing, and the printing ink uses acid-resistant ink;
[0018] (3) After the ink is dry, put it vertically into a corrosion box filled with corrosive solution and soak for 25 minutes. The composition and proportion of the corrosive solution are prepared by weight percentage, water: 50%, sulfuric acid: 23%, hydrofluoric acid: 27%;
[0019] (4) put the corroded jade sand glass into the water tank and clean it up;
[0020] (5) put the cleaned jade sand glass into a box filled with sodium hydroxide solution and soak for 20 minutes, the concentration of sodium hydroxide solution is prepared by weight percentage, water: 75%, sod...
Embodiment 2
[0024] Taking non-patterned sand-carved glass as an example, a production method of non-printed glass, the production process steps are as follows:
[0025] (1) Wash and dry the sand sculpture glass with a cleaning machine equipped with ionized water and drying equipment;
[0026] (2) Place the cleaned sand-carved glass vertically into a corrosion box filled with corrosive liquid and soak for 25 minutes. : 27%;
[0027] (4) Put the corroded sand sculpture glass into the water tank and clean it;
[0028] (5) put the cleaned sand carving glass into a box filled with sodium hydroxide solution and soak for 20 minutes, the concentration of the sodium hydroxide solution is prepared by weight percentage, water: 75%, sodium hydroxide 25%;
[0029] (6) Put the sand sculpture glass soaked in the sodium hydroxide solution tank into the water tank for cleaning for 1 minute;
[0030] (7) remove the anti-acid corrosion ink, then put into a cleaning machine equipped with ionized water and...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com