A smooth wool yangbuck and resin technology, which is applied in the field of skin-feeling down-smooth wool yangbuck resin and its preparation, can solve the problems of unsatisfactory down-smooth wool of yangbuck, rough hand feeling of yangbuck, change of hand feeling, etc., and achieve comprehensive Good effect, unique leather feel, strong leather effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] The skin feeling down-smooth wool yamba resin provided by the present embodiment consists of 25 parts by weight of modified polyurethane resin, 25 parts by weight of methyl ethyl ketone, 25 parts by weight of toluene, 0.8 parts by weight of modified silicone, 2.5 parts by weight of foamed microspheres and 1 It consists of organic wax flakes in parts by weight.
[0023] The preparation method of the above-mentioned skin feeling down-smooth wool yambuck resin is:
[0024] 1) Mix 1 part by weight of organic wax flakes with 10 parts by weight of toluene, and heat to completely dissolve the organic wax flakes in toluene;
[0025] 2) Mix 2.5 parts by weight of foamed microspheres with 15 parts by weight of toluene, stir evenly, and filter with a 200-mesh filter;
[0026] 3) Evenly mix the mixture obtained in step 1) with the mixture obtained in step 2);
[0027] 4) Dissolve 25 parts by weight of modified polyurethane resin and 0.8 parts by weight of modified silicone in 25 ...
Embodiment 2
[0031] The skin-feeling down-smooth yamba resin provided in this embodiment consists of 35 parts by weight of modified polyurethane resin, 35 parts by weight of methyl ethyl ketone, 35 parts by weight of toluene, 1 part by weight of modified silicone, 4 parts by weight of foamed microspheres and 3 parts by weight of It consists of organic wax flakes in parts by weight.
[0032] The preparation method of the above-mentioned skin feeling down-smooth wool yambuck resin is:
[0033] 1) Mix 3 parts by weight of organic wax flakes with 10 parts by weight of toluene, and heat to completely dissolve the organic wax flakes in toluene;
[0034] 2) Mix 4 parts by weight of foamed microspheres with 25 parts by weight of toluene, stir evenly, and filter with a 200-mesh filter;
[0035] 3) Evenly mix the mixture obtained in step 1) with the mixture obtained in step 2);
[0036] 4) Dissolve 35 parts by weight of modified polyurethane resin and 1 part by weight of modified silicone in 35 pa...
Embodiment 3
[0040] The skin feeling down-smooth yamba resin provided by this embodiment consists of 30 parts by weight of modified polyurethane resin, 30 parts by weight of methyl ethyl ketone, 30 parts by weight of toluene, 0.9 parts by weight of modified silicone, 3.25 parts by weight of foamed microspheres and 1.5 parts by weight It consists of organic wax flakes in parts by weight.
[0041] The preparation method of the above-mentioned skin feeling down-smooth wool yambuck resin is:
[0042] 1) Mix 1.5 parts by weight of organic wax flakes with 10 parts by weight of toluene, and heat to completely dissolve the organic wax flakes in toluene;
[0043] 2) Mix 3.25 parts by weight of foamed microspheres with 20 parts by weight of toluene, stir evenly, and filter with a 200-mesh filter;
[0044] 3) Evenly mix the mixture obtained in step 1) with the mixture obtained in step 2);
[0045] 4) Dissolve 30 parts by weight of modified polyurethane resin and 0.9 parts by weight of modified sili...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com