Inelastic lace trimming and production method thereof
A lace and lace technology, applied in the field of warp knitting and dyeing and finishing, to achieve the effects of good stability, low price and long-term efficacy
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0048]A non-stretch lace lace, in which a lace layer is compounded on a non-stretch fabric, the lace layer is woven from nylon-polyester composite yarn and modified nylon yarn, and the mass ratio of nylon-polyester composite yarn to modified nylon yarn is 1:1. The weaving technology of its lace is an existing mature technology.
[0049] A kind of modified nylon yarn, its raw material mass percentage is:
[0050] Coir Modifier 1%
[0051] Nylon chips 99%
[0052] A kind of preparation method of modified nylon yarn, its concrete steps are:
[0053] (1) Raw material pretreatment:
[0054] Coconut shells were dried at 70°C for 4 hours to obtain treated coconut shells;
[0055] (2) Carbonization treatment:
[0056] Carry out carbonization to obtain modified coconut shell powder with the processed coconut shell that step (1) obtains;
[0057] The carbonization process is to use a quartz tube furnace to carry out the segmented carbonization of coconut shells: the temperature ri...
Embodiment 2
[0075] A non-stretch lace lace, in which a lace layer is compounded on a non-stretch fabric, the lace layer is woven from nylon-polyester composite yarn and modified nylon yarn, and the mass ratio of nylon-polyester composite yarn to modified nylon yarn is 1:1. The weaving technology of its lace is an existing mature technology.
[0076] A kind of modified nylon yarn, its raw material mass percentage is:
[0077] Coir Modifier 2%
[0078] Nylon chips 98%
[0079] A kind of preparation method of modified nylon yarn, its concrete steps are:
[0080] (1) Raw material pretreatment:
[0081] Coconut shells were dried at 70°C for 4 hours to obtain treated coconut shells;
[0082] (2) Carbonization treatment:
[0083] Carry out carbonization to obtain modified coconut shell powder with the processed coconut shell that step (1) obtains;
[0084] The carbonization process is to use a quartz tube furnace to carry out the segmented carbonization of coconut shells: the temperature r...
Embodiment 3
[0100] A non-stretch lace lace, in which a lace layer is compounded on a non-stretch fabric, the lace layer is woven from nylon-polyester composite yarn and modified nylon yarn, and the mass ratio of nylon-polyester composite yarn to modified nylon yarn is 1:1. The weaving technology of its lace is an existing mature technology.
[0101] A kind of modified nylon yarn, its raw material mass percentage is:
[0102] Coir Modifier 3%
[0103] Nylon chips 97%
[0104] A kind of preparation method of modified nylon yarn, its concrete steps are:
[0105] (1) Raw material pretreatment:
[0106] Coconut shells were dried at 70°C for 4 hours to obtain treated coconut shells;
[0107] (2) Carbonization treatment:
[0108] Carry out carbonization to obtain modified coconut shell powder with the processed coconut shell that step (1) obtains;
[0109] The carbonization process is to use a quartz tube furnace to carry out the segmented carbonization of coconut shells: the temperature r...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com