A viscose fiber, same-bath dyeing technology, applied in the direction of dyeing method, fiber type, fiber treatment, etc., can solve the problems of complex production process, unstable process control, insufficient energy saving, etc., and achieve simple production process, energy saving, process Controlling stable effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0012] A kind of bath dyeing method of spandex and viscose fiber, comprises the steps:
[0013] 1) Take 2 parts by mass of viscose fiber and 3 parts by mass of spandex blended yarn to weave knitted fabric;
[0014] 2) Put the knitted fabric into the overflow dyeing machine, add water, then add 3g / L chelating agent and 3g / L isopropanolamine in turn, adjust the pH to 5, heat up to 60°C, run for 20 minutes, add reactive dyes , run for 30 minutes, add cationic dyes, run for 30 minutes, add 35g / L Yuanming powder, run for 25 minutes, raise the temperature to 90°C at 5°C / min, run for 1 hour, cool down to 35°C, drain, then drain at 75°C Wash in hot water at ℃ for 30 minutes;
[0015] 3) Put the dyed knitted fabric into 35°C water, add 3g / L acid soaping agent and 4g / L hydroxypropyl methylcellulose in sequence, heat up to 90°C, run for 40 minutes, enter cold water, overflow , cooled to 15°C, drained, and then washed with cold water for 20 minutes.
Embodiment 2
[0017] A kind of bath dyeing method of spandex and viscose fiber, comprises the steps:
[0018] 1) Take 2 parts by mass of viscose fiber and 3 parts by mass of spandex blended yarn to weave knitted fabric;
[0019] 2) Put the knitted fabric into the overflow dyeing machine, add water, then add 2g / L chelating agent and 2g / L isopropanolamine in sequence, adjust the pH to 4, heat up to 60°C, run for 20 minutes, add reactive dyes , run for 30 minutes, add cationic dyes, run for 30 minutes, add 30g / L Yuanming powder, run for 25 minutes, raise the temperature to 90°C at 5°C / min, run for 1 hour, cool down to 35°C, drain water, and then use 75°C Wash in hot water at ℃ for 30 minutes;
[0020] 3) Put the dyed knitted fabric into 35°C water, add 2g / L acid soaping agent and 3g / L hydroxypropyl methylcellulose in sequence, heat up to 90°C, run for 40 minutes, enter cold water, overflow , cooled to 15°C, drained, and then washed with cold water for 20 minutes.
Embodiment 3
[0022] A kind of bath dyeing method of spandex and viscose fiber, comprises the steps:
[0023] 1) Take 2 parts by mass of viscose fiber and 3 parts by mass of spandex blended yarn to weave knitted fabric;
[0024] 2) Put the knitted fabric into the overflow dyeing machine, add water, then add 2.3g / L chelating agent and 2.3g / L isopropanolamine in sequence, adjust the pH to 4.5, heat up to 60°C, run for 20 minutes, add Reactive dyes, run for 30 minutes, add cationic dyes, run for 30 minutes, add 33g / L sodium sulfate, run for 25 minutes, heat up to 90°C at 5°C / min, run for 1 hour, cool down to 35°C, drain, and then Wash in hot water at 75°C for 30 minutes;
[0025] 3) Put the dyed knitted fabric into 35°C water, add 2.3g / L acid soaping agent and 3.4g / L hydroxypropyl methylcellulose in sequence, raise the temperature to 90°C, run for 40 minutes, enter cold water, Overflow, cool down to 15°C, drain, then add cold water to wash for 20 minutes.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com