A kind of wall thermal insulation paste
A technology for thermal insulation and slurry, applied in the field of construction slurry, can solve problems such as low fire rating, hollowing, fire accidents, etc., and achieve the effects of easy procurement, simple preparation and use, and remarkable thermal insulation effect.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] 35kg of bentonite, 20kg of vermiculite powder, 20kg of perlite, 15kg of powdered lime, 10kg of calcium hydroxide, 10kg of white cotton, 8kg of aluminum silicate fiber, 3kg of silicon dioxide, 3kg of fast T, 10kg of ammonium phosphate, and 20kg of sawdust powder.
[0017] The above-mentioned bentonite, vermiculite powder, perlite, powdery lime, calcium hydroxide, white cotton, silicon dioxide, ammonium phosphate and sawdust powder are put into a mixer and stirred for 15-25 minutes until they are evenly stirred to obtain a mixed slurry A, which is packaged and put into storage ; Pack fast T and aluminum silicate fiber separately to obtain mixed slurry B.
Embodiment 2
[0019] 25kg of bentonite, 15kg of vermiculite powder, 20kg of perlite, 15kg of powdered lime, 8kg of calcium hydroxide, 8kg of white cotton, 8kg of aluminum silicate fiber, 3kg of silicon dioxide, 3kg of fast T, 8kg of calcium silicate, and 15kg of sawdust powder.
[0020] The above-mentioned bentonite, vermiculite powder, perlite, powdery lime, calcium hydroxide, white cotton, silicon dioxide, calcium silicate and sawdust powder were put into a mixer and stirred for 15-25 minutes until they were evenly stirred to obtain a mixed slurry A, which was packed into library; the fast T and aluminum silicate fibers are packaged separately to obtain the mixed slurry B.
Embodiment 3
[0022] 20kg of bentonite, 10kg of vermiculite powder, 15kg of perlite, 10kg of powdered lime, 5kg of calcium hydroxide, 5kg of white cotton, 5kg of aluminum silicate fiber, 2kg of silicon dioxide, 2kg of fast T, 5kg of aluminum phosphate, and 15kg of sawdust powder.
[0023] The above-mentioned bentonite, vermiculite powder, perlite, powdery lime, calcium hydroxide, white cotton, silicon dioxide, aluminum phosphate and sawdust powder are put into a mixer and stirred for 15-25 minutes until they are evenly stirred to obtain a mixed slurry A, which is packaged and stored ; Pack fast T and aluminum silicate fiber separately to obtain mixed slurry B.