A manufacturing method and micrometer technology, applied to micrometers, manufacturing tools, furnace types, etc., can solve the problems of unstable measurement accuracy, low anvil hardness, and low dimensional stability of micrometer components, so as to improve dimensional stability and hardness, Effect of low cost and improved hardenability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] A manufacturing method of a micrometer, which includes the following steps:
[0031] (1) Preparation of micrometer materials:
[0032] The mass percentages of the micrometer blank components are: C: 1.00%, Cr: 1.45%, Co: ≦1.00%, Mn: ≦0.40%, Si: ≦0.35%, S: ≦0.03%, P: ≦0.03%, and more The amount is Fe;
[0033] (2) Forging of blank:
[0034] The billet is heated to the initial forging temperature in an intermediate frequency induction heating furnace, and then the heated billet is placed in a rolling mill and rolled into a micrometer blank by a rolling die;
[0035] (3) Normalizing treatment of forging blanks:
[0036] The forging blank obtained in step (2) is normalized, the normalizing temperature is 830°C, the temperature is kept for 7 hours, and then it is discharged from the furnace and air-cooled to room temperature;
[0037] (4) Spheroidizing annealing treatment of forging blank:
[0038] Spheroidizing annealing is performed on the forging blank obtained in step (3), the annea...