An ultrasonic and leaching technology, applied in the field of potassium extraction from potassium feldspar, can solve the problems of high equipment requirements, equipment corrosion, environmental pollution, etc., and achieve the effects of promoting acid dissolution, saving production costs, and being environmentally friendly.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] This embodiment includes the following steps:
[0028] (1) Grinding the potassium feldspar ore to a fineness of about 150 mesh;
[0029] (2) Add 10 mL of mixed acid solution per gram of potassium feldspar, and mix evenly, wherein the concentration of phosphoric acid is 60%, and the concentration of oxalic acid is 0.2 mol / L;
[0030] (3) Leach the mixture obtained in step (2) under normal pressure: the reaction temperature is: 50° C., and the reaction time is 22 hours; during the reaction, ultrasonic-assisted leaching is carried out to the reaction mixture, and 40 kHz ultrasonic treatment is adopted, and the ultrasonic power is 100 W. Add water to the original volume, ultrasonic time 1h;
[0031] (4) Adding distilled water with the same volume as the mixed solution to the reacted material, leaching, and separating the solid and liquid to obtain a soluble potassium solution.
[0032] The test results show that the leaching rate of potassium after the reaction is 50.8%. ...
Embodiment 2
[0034] This embodiment includes the following steps:
[0035] (1) Grinding the potassium feldspar ore to a fineness of about 150 mesh;
[0036] (2) Add 10 mL of mixed acid solution per gram of potassium feldspar, mix well, wherein the concentration of phosphoric acid is 60%, and the concentration of oxalic acid is 0.2 mol / L;
[0037] (3) Leach the mixture obtained in step (2) under normal pressure: the reaction temperature is: 60°C, and the reaction time is 22h; during the reaction, ultrasonic-assisted leaching is carried out to the reaction mixture, and 40kHz ultrasonic treatment is adopted, and the ultrasonic power is 100W. Add water to the original volume, ultrasonic time 1h;
[0038] (4) Adding distilled water with the same volume as the mixed solution to the reacted material, leaching, and separating the solid and liquid to obtain a soluble potassium solution.
[0039] The test results show that the leaching rate of potassium after the reaction is 41.0%.
Embodiment 3
[0041] This embodiment includes the following steps:
[0042] (1) Grinding the potassium feldspar ore to a fineness of about 150 mesh;
[0043] (2) Add 10 mL of mixed acid solution per gram of potassium feldspar, mix well, wherein the concentration of phosphoric acid is 60%, and the concentration of oxalic acid is 0.2 mol / L;
[0044] (3) Leach the mixture obtained in step (2) under normal pressure: the reaction temperature is: 50° C., and the reaction time is 30 h; during the reaction, ultrasonic-assisted leaching is carried out to the reaction mixture, and 40 kHz ultrasonic treatment is adopted, and the ultrasonic power is 100 W. Add water to the original volume, ultrasonic time 1h;
[0045] (4) Adding distilled water with the same volume as the mixed solution to the reacted material, leaching, and separating the solid and liquid to obtain a soluble potassium solution.
[0046] The test results show that the leaching rate of potassium after the reaction is 54.0%.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com