A method of using waste stone powder to prepare self-leveling mortar
What is Al technical title?
Al technical title is built by PatSnap Al team. It summarizes the technical point description of the patent document.
A technology for self-leveling mortar and waste stone powder is applied in the field of building materials, which can solve the problems of insufficient function and easy segregation and bleeding, and achieve the effects of reducing segregation and bleeding, improving uniformity and avoiding concentrated growth.
Active Publication Date: 2018-04-13
GUILIN UNIVERSITY OF TECHNOLOGY
View PDF6 Cites 0 Cited by
Summary
Abstract
Description
Claims
Application Information
AI Technical Summary
This helps you quickly interpret patents by identifying the three key elements:
Problems solved by technology
Method used
Benefits of technology
Problems solved by technology
However, waste stone powder is only used in ordinary mortar concrete, and self-leveling mortar is a special mortar with high fluidity, which is very easy to segregate and bleed. A lot of research basically adopts the method of increasing the specific gravity of fine powder materials or adding thickeners. Improve the consistency and solve the problem of segregation and bleeding. The fineness of waste stone powder can meet the requirements. It is a relatively fine powder with a significant thickening effect. When it is used in ordinary mortar, this effect cannot be fully exerted, but for self-leveling Mortar, the effect is very obvious
[0005] At present, there is no report on using waste stone powder instead of river sand to make self-leveling mortar
Method used
the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more
Examples
Experimental program
Comparison scheme
Effect test
Embodiment 1
[0025] Mix 385g ordinary 42.5 portland cement, 210g early strength cement, 105g fly ash, 115g waste stone powder and 655g fine river sand, then add 0.42g thickener hydroxypropyl methyl cellulose ether, 0.36g early Strong agent aluminum sulfate, 0.3g silicone defoamer and 1.3g retarder sodium gluconate, after stirring evenly, gradually add water according to the water-binder ratio of 0.4, after stirring for 1 minute, add 1.7g polycarboxylate superplasticizer, continue Stir, stir evenly, let stand for 30 seconds, then stir quickly for 1 minute to prepare self-leveling mortar.
[0026] The waste stone powder is collected in the production of machine-made sand, and the fineness is less than 75 μm.
[0027] The fineness modulus of the fine river sand is 2.0.
[0028] The properties of the prepared self-leveling mortar have been tested. The initial fluidity and 20-minute fluidity can reach 143mm and 140mm respectively. 6.8MPa and 30MPa.
Embodiment 2
[0030] Mix 350g of ordinary 42.5 Portland cement, 210g of early strength cement, 140g of fly ash, 154g of waste stone powder, and 616g of fine river sand, and then add 0.35g of thickener hydroxyethyl methyl cellulose ether, 0.42g of early Strong agent lithium carbonate, 0.3g high-grade fatty acid ester defoamer and 1.2g retarder tartaric acid, after stirring evenly, add water gradually according to the water-binder ratio of 0.4, stir for 1 minute, add 1.6g naphthalene-based water reducer, and continue stirring , Stir evenly, let it stand for 30 seconds, and then stir quickly for 1 minute to prepare self-leveling mortar.
[0031] The waste stone powder is collected in the production of machine-made sand, and the fineness is less than 75 μm.
[0032] The fineness modulus of the fine river sand is 2.0.
[0033] The properties of the prepared self-leveling mortar have been tested. The initial fluidity and 20-minute fluidity reach 141mm and 139mm respectively, the flexural and com...
the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More
PUM
Property
Measurement
Unit
compressive strength
aaaaa
aaaaa
compressive strength
aaaaa
aaaaa
Login to View More
Abstract
The invention discloses a preparation method of self-leveling mortar using waste stone powder. The method includes: (1) proportioning raw materials, to be specific, proportioning raw materials including, by weight, 24% to 28% of ordinary Portland cement 42.5, 12% to 17% of high early strength cement, 8% to 12% of fly ash, 48% to 50% of fine river sand, 8% to 10% of the waste stone powder, 0.02% to 0.04% of thickener, 0.02% to 0.04% of early strength agent, 0.02% to 0.04% of defoaming agent, 0 .1% to 0.12% of retarder and 0.1% to 0.13% of water reducing agent, with the raw materials adding up 100%; (2) uniformly mixing the ordinary Portland cement, the high early strength cement, the fly ash, the waste stone powder and the fine river sand, adding sequentially the thickener, the early strength agent, the defoaming agent and the retarder, and stirring evenly; according to the water-binder ratio of 0.4, gradually adding water, performing stirring for 1 minute before adding the water reducing agent, performing uniform mixing and standing for 30 seconds, and then performing quick stirring for 1 minute to obtain the self-leveling mortar. The use of the method costs less, improves stability of the mortar, increases early strength of the mortar, and solves a large number of environmental problems caused by the waste stone powder.
Description
technical field [0001] The invention relates to the technical field of building materials, in particular to a method for preparing self-leveling mortar by using waste stone powder. Background technique [0002] Self-leveling mortar is a dry-mixed powdery material composed of a variety of active ingredients. It can be used after mixing with water on site. After a little spreading with a scraper, a high-level base surface can be obtained. It has high early strength and can improve construction efficiency. It is suitable for Fine leveling of concrete floors and all flooring materials are widely used in civil and commercial buildings. [0003] At present, my country's self-leveling mortar technology is not yet fully mature, and it is still facing problems such as poor work performance, low early strength and low utilization rate of waste residue. At present, self-leveling mortar basically uses fine river sand as aggregate, and since river sand mining has caused serious environm...
Claims
the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More
Application Information
Patent Timeline
Application Date:The date an application was filed.
Publication Date:The date a patent or application was officially published.
First Publication Date:The earliest publication date of a patent with the same application number.
Issue Date:Publication date of the patent grant document.
PCT Entry Date:The Entry date of PCT National Phase.
Estimated Expiry Date:The statutory expiry date of a patent right according to the Patent Law, and it is the longest term of protection that the patent right can achieve without the termination of the patent right due to other reasons(Term extension factor has been taken into account ).
Invalid Date:Actual expiry date is based on effective date or publication date of legal transaction data of invalid patent.