A kind of aluminum alloy rod and its preparation method and the preparation method of aluminum alloy wire
An aluminum alloy rod and aluminum alloy monofilament technology, applied in the field of aluminum alloy rod and its preparation, can solve the problem of lack of bending performance and impact resistance, unreachable elongation and tensile strength, poor creep resistance, etc. problems, to achieve the effect of improving bending performance and elongation, increasing elongation, and good tensile strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] For a 3000kg aluminum alloy rod, the weight percentage of each component is shown in the table below:
[0031] components
Fe
Mg
Zr
Cu
Re
Mn+Ni
Al
Impurities
Weight (Kg)
45
15
/
4.8
/
/
2933.7
1.5
weight percentage (%)
1.5
0.5
/
0.16
/
/
97.79
0.05
[0032] In the aluminum alloy rods mentioned in the above table, due to the addition of 0.16% Cu by weight, although the electrical conductivity of the aluminum alloy rods has decreased slightly, it has greatly improved the strength, heat resistance temperature and wire drawing of the aluminum alloy rods. Effect.
[0033] A method for preparing the above-mentioned aluminum alloy rod, using the following steps:
[0034] (1) Alloy treatment: Add the aluminum liquid of the above weight into the holding furnace and heat the aluminum liquid so that the temperature of the aluminum liquid in the holding furnace is controlled at...
Embodiment 2
[0043] For a 3000kg aluminum alloy rod, the weight percentage of each component is shown in the table below:
[0044] components
Fe
Mg
Zr
Cu
Re
Mn+Ni
Al
Impurities
Weight (Kg)
10.5
9
/
4.8
/
0.9
2973.6
1.2
weight percentage (%)
0.35
0.3
/
0.16
/
0.03
99.12
0.04
[0045] In the aluminum alloy rods mentioned in the above table, the Mn and Ni of the above-mentioned weights are added preferentially. Although Mn will cause a significant decrease in the conductivity of the aluminum alloy rods, it can improve the strength of the aluminum alloy rods and effectively refine the recrystallized grains. grains, which improves the toughness of the aluminum alloy rod to a certain extent; the addition of Ni will generate metal compounds such as aluminum nickel AlNi3 in the aluminum alloy rod, which are distributed in the matrix grain boundary in the form of a dispersed phase, and have the ...
Embodiment 3
[0056] For a 3000kg aluminum alloy rod, the weight percentage of each component is shown in the table below:
[0057] components
Fe
Mg
Zr
Cu
Re
Mn+Ni
Al
Impurities
Weight (Kg)
8.4
7.5
1.2
4.2
/
0.84
2976.06
1.8
weight percentage (%)
0.28
0.25
0.04
0.14
/
0.028
99.202
0.06
[0058] In the aluminum alloy rods mentioned in the table above, adding Zr with the above-mentioned weight preferentially results in a significant decrease in the electrical conductivity of the aluminum alloy rod, but it is very effective in improving the heat resistance of the aluminum alloy rod.
[0059] A method for preparing the above-mentioned aluminum alloy rod, using the following steps:
[0060] (1) Alloy treatment: Add the aluminum liquid of the above weight into the holding furnace and heat the aluminum liquid so that the temperature of the aluminum liquid in the holding furnace is controlled a...
PUM
| Property | Measurement | Unit |
|---|---|---|
| tensile strength | aaaaa | aaaaa |
| elastic limit | aaaaa | aaaaa |
| tensile strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More