A kind of preparation method of cotton pulp for high-strength filter paper
A cotton pulp, high-strength technology, applied in the field of pulp manufacturing, can solve the problems of filter cleaning ability decline, moisture absorption performance and strength influence, automobile engine failure, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] Embodiment 1, a kind of preparation method of cotton pulp for high-strength filter paper, comprises the following steps:
[0036] A. Cotton opening:
[0037] With the air-dried pulp 2640Kg / ball or the absolute-dried pulp 2401Kg / ball as the basic unit, it is manually separated according to the requirements of the feeding thickness ≤ 10cm and put into the cotton opener. The feeding time of each basic unit is ≥ 30min, and then two series of seven The roller opener and three five-roller openers in series are all turned on, so that the pulp output by the opener passes through in sequence;
[0038] The frequency of the opening fan on the opener is set to 50 Hz / min, and cotton linters are used for air-dried pulp or absolute-dried pulp.
[0039] B. Alkali
[0040] Prepare alkali solution with the standard of 9600L / ball (relative to air-dried pulp 2640Kg / ball or absolute dry pulp 2401Kg / ball);
[0041] The concentration of NaOH in the alkali solution is 39g / L, and the tempera...
Embodiment 2
[0064] Embodiment 2, a kind of preparation method of cotton pulp for high-strength filter paper, comprises the following steps:
[0065] A. Cotton opening:
[0066] With the air-dried pulp 2650Kg / ball or the absolute-dried pulp 2411Kg / ball as the basic unit, it is manually separated according to the requirements of the feeding thickness ≤ 10cm and put into the cotton opener. The feeding time of each basic unit is ≥ 30 minutes, and then two series-connected The seven-roller opener and three five-roller openers in series are all turned on, so that the pulp output by the opener passes through in sequence;
[0067] The frequency of the opening fan on the opener is set to 50 Hz / min, and cotton linters are used for air-dried pulp or absolute-dried pulp.
[0068] B. Alkali
[0069] Prepare alkali solution with the standard of 9600L / ball (relative to air-dried pulp 2650Kg / ball or absolute dry pulp 2411Kg / ball);
[0070] The concentration of NaOH in the alkali solution is 40g / L, and...
Embodiment 3
[0093] Embodiment 3, a kind of preparation method of cotton pulp for high-strength filter paper, comprises the following steps:
[0094] A. Cotton opening:
[0095] With the air-dried pulp 2660Kg / ball or the absolute-dried pulp 2421Kg / ball as the basic unit, it is manually separated according to the requirements of the feeding thickness ≤ 10cm and put into the cotton opener. The feeding time of each basic unit is ≥ 30min, and then two series-connected seven The roller opener and three five-roller openers in series are all turned on, so that the pulp output by the opener passes through in sequence;
[0096] The frequency of the opening fan on the opener is set to 50 Hz / min, and cotton linters are used for air-dried pulp or absolute-dried pulp.
[0097] B. Alkali
[0098] Prepare alkali solution with the standard of 9600L / ball (relative to air-dried pulp 2660Kg / ball or absolute dry pulp 2421Kg / ball);
[0099] The concentration of NaOH in the alkali solution is 41g / L, and the ...
PUM
| Property | Measurement | Unit |
|---|---|---|
| degree of polymerization | aaaaa | aaaaa |
| whiteness | aaaaa | aaaaa |
| degree of polymerization | aaaaa | aaaaa |