Non-woven fabric applied to paper diaper core and production method thereof
A production method and technology of non-woven fabrics, which are applied to complete sets of equipment for producing artificial threads, non-woven fabrics, and elongation of fabrics, etc., can solve problems such as inability to make ultra-thin cores, and achieve excellent water-locking effect and comfort. High, good diversion effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] Embodiment 1: the preparation of fluffy flow-guiding non-woven fabric
[0036] (1) mixing the raw materials to prepare a compound, the raw materials are calculated in the following percentages by weight: polypropylene is 92%, and propylene-based plasticizer is 8%;
[0037] (2) extruding and melting the mixture in a screw extruder to form a hot melt, the temperature of the screw is 260°C, and the temperature of the hot melt is 250°C;
[0038] (3) Filtrate and measure the hot melt through a filter and a metering pump. The filtration and metering are carried out at a temperature of 220 ° C and a pressure of 3 MPa; the hot melt is spun, and the spinning is through 0.4 ~ The spinneret with 0.8mm aperture is sprayed out, and the spinneret temperature is 250°C;
[0039] (4) Cool the filaments ejected in step (3) in the cooling wind box to obtain primary filaments through side cooling air. The fiber is obtained by drafting, and the fiber is divided into a web to form a web by...
Embodiment 2
[0043] Embodiment 2: the preparation of fluffy flow-guiding non-woven fabric
[0044] (1) mixing the raw materials to obtain a compound, the raw materials are calculated in the following percentages by weight: 96% for polypropylene and 4% for propylene-based plasticizer;
[0045] (2) extruding and melting the mixture in a screw extruder to form a hot melt, the temperature of the screw is 280°C, and the temperature of the hot melt is 270°C;
[0046] (3) Filtrate and measure the hot melt through a filter and a metering pump. The filtration and metering are carried out at a temperature of 250 ° C and a pressure of 15 MPa; the hot melt is sprayed, and the spinning is through 0.4 ~ The spinneret with 0.8mm aperture is sprayed out, and the spinneret temperature is 280°C;
[0047] (4) Cool the filaments ejected in step (3) in the cooling wind box to obtain primary filaments through side cooling air. The fiber is obtained by drafting, and the fiber is divided into a web to form a we...
Embodiment 3
[0051] Embodiment 3: the preparation of fluffy flow-guiding non-woven fabric
[0052] (1) mixing the raw materials to obtain a compound, the raw materials are calculated in the following percentages by weight: 95% for polypropylene and 5% for propylene-based plasticizer;
[0053] (2) extruding and melting the mixture in a screw extruder to form a hot melt, the temperature of the screw is 260°C, and the temperature of the hot melt is 250°C;
[0054] (3) Filtrate and measure the hot melt through a filter and a metering pump. The filtration and metering are carried out at a temperature of 230 ° C and a pressure of 8 MPa; the hot melt is sprayed, and the spinning is through 0.4 ~ The spinneret with 0.8mm aperture is sprayed out, and the spinneret temperature is 260°C;
[0055] (4) Cool the filaments ejected in step (3) in the cooling wind box to obtain primary filaments through side cooling air. The fiber is obtained by drafting, and the fiber is divided into a web to form a web...