A kind of fluorescent cloth and preparation method thereof
A fluorescent coating and fluorescent technology, which is applied in textiles and papermaking, etc., can solve the problems of unsightly effects on fluorescent effects, uneven application of fluorescent particles, and inability to provide warning effects, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] Example 1: Preparation of a fluorescent fabric
[0027] Preparation of water-based polyurethane gold oil A: mixed configuration of 94% of water-based polyurethane resin, 3% of propylene glycol, 2.5% of defoaming and thickening aids, and 0.5% of organic amine.
[0028] Preparation of water-based polyurethane gold oil B: water-based polyurethane resin 91%, propylene glycol 5%, defoaming and thickening aid 3.5%, organic amine 0.5% mixed configuration.
[0029] Preparation of the first fluorescent paint: Mix fluorescent particles with a particle size of 20-25um in a propylene glycol solution, ultrasonically disperse to obtain a solution containing fluorescent particles, and then mix the solution containing fluorescent particles with water-based polyurethane gold oil B, and uniformly disperse at high speed , the first fluorescent paint is obtained. In the first fluorescent paint: the mass ratio of fluorescent particles, propylene glycol solution, and water-based polyurethan...
Embodiment 2
[0037] Example 2 Preparation of a fluorescent fabric
[0038] Preparation of water-based polyurethane gold oil A: water-based polyurethane resin 95%, ethanol 2.5%, defoaming and thickening aid 2%, organic amine 0.5% mixed configuration.
[0039] Preparation of water-based polyurethane gold oil B: water-based polyurethane resin 90%, ethanol 7%, defoaming and thickening aid 2.5%, organic amine 0.5% mixed configuration.
[0040] Preparation of the first fluorescent paint: Mix fluorescent particles with a particle size of 20-25um in an ethanol solution, ultrasonically disperse to obtain a solution containing fluorescent particles, and then mix the solution containing fluorescent particles with water-based polyurethane gold oil B, and uniformly disperse at high speed , the first fluorescent paint is obtained.
[0041] In the first fluorescent paint: the mass ratio of fluorescent particles, ethanol solution, and water-based polyurethane is 0.2:7:50.
[0042] Preparation of the sec...
Embodiment 3
[0048] Example 3 Preparation of a fluorescent fabric
[0049] Preparation of water-based polyurethane gold oil A: water-based polyurethane resin 95%, ethanol 2.5%, defoaming and thickening aid 2%, organic amine 0.5% mixed configuration.
[0050] Preparation of water-based polyurethane gold oil B: water-based polyurethane resin 87%, dipropylene glycol methyl ether 8.5%, defoaming and thickening aid 4%, organic amine 0.5% mixed configuration.
[0051] Preparation of water-based polyurethane gold oil C: water-based polyurethane resin 93%, dipropylene glycol butyl ether 3.3%, defoaming and thickening aid 3%, organic amine 0.7% mixed configuration.
[0052] Preparation of the first fluorescent paint: Mix fluorescent particles with a particle size of 20-25um in an ethanol solution, ultrasonically disperse to obtain a solution containing fluorescent particles, and then mix the solution containing fluorescent particles with water-based polyurethane gold oil B, and uniformly disperse a...
PUM
| Property | Measurement | Unit |
|---|---|---|
| thickness | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |