Preparation method of superfine wool fiber tops
A wool fiber and wool top technology, which is applied in the field of preparation of ultra-fine wool fiber tops, can solve problems such as easy moths, and achieve the effect of simple preparation method, good hand feeling and physical properties
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A method for preparing a superfine wool fiber top, comprising the steps of cleaning raw wool, wool blending, carding and needle combing; specifically comprising the following steps:
[0019] 1) Washing of raw wool: select sheep wool and put it into the washing tank for cleaning, first soak for 20-30 minutes, after soaking, manually separate the wool by hand, and wash for 3-5 times until the washing water is clear;
[0020] 2) Wool blending: the raw wool is cleaned and rehydrated at 10.65, and blended hair oil and antistatic agent are added when blending the wool;
[0021] 3) Combing: the speed of combing sliver is 60-80m / min, and the weight of sliver is 15-17g / m±2;
[0022] 4) Needle combing includes front needle combing, combing and back needle process;
[0023] The traction gauge of the preceding needle comb is 32mm, the speed is 70m / min, and the sliver weight is 150g / m, the combing traction gauge is 30mm, the speed is 60m / min, and the sliver weight is 10g / m , the b...
Embodiment 2
[0028] A method for preparing a superfine wool fiber top, comprising the steps of cleaning raw wool, wool blending, carding and needle combing; specifically comprising the following steps:
[0029] 1) Washing of raw wool: select sheep wool and put it in the washing tank for cleaning, firstly soak it for 25 minutes, after soaking, manually separate the wool by hand, and wash it 4 times until the washing water is clear;
[0030] 2) Wool blending: the raw wool is cleaned and rehydrated at 10.65, and blended hair oil and antistatic agent are added when blending the wool;
[0031] 3) Combing: the speed of combing sliver is 70m / min, and the weight of sliver is 16g / m±2;
[0032] 4) Needle combing includes front needle combing, combing and back needle process;
[0033] The traction gauge of the preceding needle comb is 35mm, the speed is 80m / min, and the sliver weight is 18g / m, the combing traction gauge is 31mm, the speed is 70m / min, and the sliver weight is 12g / m , the back needle...
Embodiment 3
[0038] A method for preparing a superfine wool fiber top, comprising the steps of cleaning raw wool, wool blending, carding and needle combing; specifically comprising the following steps:
[0039] 1) Washing of raw wool: select sheep wool and put it in the washing tank for cleaning, first soak for 30 minutes, after soaking, manually separate the wool by hand, and wash it 5 times until the washing water is clear;
[0040] 2) Wool blending: the raw wool is cleaned and rehydrated at 10.65, and blended hair oil and antistatic agent are added when blending the wool;
[0041] 3) Combing: the speed of combing sliver is 80m / min, and the weight of sliver is -17g / m±2;
[0042] 4) Needle combing includes front needle combing, combing and back needle process;
[0043] The traction gauge of the preceding needle comb is 38mm, the speed is 90m / min, and the sliver weight is 20g / m, the combing traction gauge is 32mm, the speed is 80m / min, and the sliver weight is 15g / m , the back needle tra...
PUM