A technology of photocatalyst and nitrogen vacancies, which is applied in the direction of physical/chemical process catalysts, chemical instruments and methods, hydrogen, etc., can solve problems such as reducing the band gap value and increasing light absorption capacity, and achieves simple preparation methods and high photocatalytic decomposition of aquatic products. Hydrogen, the effect of increasing the hydrogen evolution rate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] Put 1 g of melamine in a covered crucible and calcinate at 550°C for 4 hours at a heating rate of 2.3°C / min. After cooling to room temperature, wash with water and alcohol for three times to collect the precipitate, and dry it in an oven at 60°C for 12 hours to obtain the basic g-C 3 N 4 Photocatalytic material 1.
Embodiment 2
[0039] Grind and mix 1g of melamine with 7wt.% oxalodihydrazine, then place it in a covered crucible and calcinate at 550°C for 4h at a heating rate of 2.3°C / min, after cooling to room temperature, wash with water and alcohol for three times to collect the precipitate , dried in an oven at 60°C for 12h to obtain nitrogen vacancy modified g-C 3 N 4 Photocatalytic material 2.
Embodiment 3
[0041] Put 1 g of melamine in a covered crucible and calcinate at 550 °C for 4 h at a heating rate of 2.3 °C / min. After cooling to room temperature, wash with water and alcohol for three times to collect the precipitate, and dry it in an oven at 60 °C for 12 h. The dried powder is transferred to a 50mL high-pressure reactor with a stainless steel substrate, and 35mL of dilute ammonia is added in the reactor. The mass percentage of ammonia is 1%. After ultrasonication in an ultrasonic machine for 30 minutes, the Transfer the reaction kettle to an oven at 160°C for 4 hours. After cooling to room temperature, wash with water and alcohol for three times to collect the precipitate, and dry it in an oven at 60°C for 12 hours to obtain hydroxyl-modified g-C 3 N 4 Photocatalytic materials3.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com