Benzoxazine, method for its preparation, coating, and method for forming a coating on a substrate surface

A benzoxazine and substrate surface technology, applied in the field of benzoxazine and its preparation, can solve the problems of polluting the environment, affecting the national economy, restricting the normal operation of industries, etc., and achieve excellent corrosion resistance

Active Publication Date: 2021-12-28
XIAMEN UNIV
View PDF13 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The loss due to corrosion cannot be ignored. It affects the national economy, restricts the normal operation of the industry, and even causes catastrophic accidents, pollutes the environment, consumes resources, etc.
[0003] At present, researchers have explored many methods of metal anti-corrosion technology, among which, coating organic coatings on metal surfaces is a simple and effective strategy

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Benzoxazine, method for its preparation, coating, and method for forming a coating on a substrate surface
  • Benzoxazine, method for its preparation, coating, and method for forming a coating on a substrate surface
  • Benzoxazine, method for its preparation, coating, and method for forming a coating on a substrate surface

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0036] [The preparation method of benzoxazine]

[0037] In some embodiments, the preparation method of benzoxazine comprises the following steps: step S1, dissolving curcumin, paraformaldehyde or formaldehyde in the first organic solvent to obtain the first solution; step S2, obtaining the first solution from step S1 Add the amine compound and the second organic solvent to the first solution, then react at 20-180°C for 1-48h, cool down after the reaction, remove the excess first organic solvent and the second organic solvent by rotary evaporation, and obtain the benzoxan A concentrated solution of oxazine; wherein, the amine compound includes a primary amine group.

[0038] The preparation method of the benzoxazine of the present application has simple synthesis steps and processes, mild reaction conditions, and simple and easy operation.

[0039] In some embodiments, the amine compound is a silane coupling agent containing primary amine groups. In some embodiments, the silane...

Embodiment 1

[0062] Weigh (0.01mol, 3.68g) curcumin, (0.04mol, 1.22g) paraformaldehyde in a 250mL three-necked flask, add 25mL of methanol, ultrasonically disperse, so that curcumin is fully dissolved; then add (0.04mol, 4.42 g) γ-Aminopropyltriethoxysilane and 100mL of dimethyl sulfoxide were reacted in an oil bath at 80°C for 6h; Add it to petroleum ether solution to obtain a viscous liquid, and obtain a concentrated liquid after separation, which is the benzoxazine monomer.

[0063] Dissolve the benzoxazine monomer in chloroform, and then spin-coat it on a clean glass or carbon steel surface for curing. The curing process is as follows: first cure at 60°C for 1 hour, then cure at 180°C for 2 hours, Then it was cured at 200°C for 2 hours, and finally at 220°C for 2 hours to obtain a coating.

Embodiment 2

[0065] Weigh (0.014mol, 5g) of curcumin, (0.197mol, 6g) of paraformaldehyde in a three-necked flask of 250mL, add 50mL of methanol, ultrasonically disperse, so that curcumin is fully dissolved; then add (0.045mol, 5g ) of γ-aminopropyltriethoxysilane and 250mL of 1,4-dioxane, react in an oil bath at 85°C for 6h; Add it dropwise into the petroleum ether solution to obtain a viscous liquid, and obtain a concentrated liquid after separation, which is the benzoxazine monomer.

[0066] Dissolve the benzoxazine monomer in chloroform, and then spin-coat it on a clean glass or carbon steel surface for curing. The curing process is as follows: first cure at 60°C for 1 hour, then cure at 180°C for 2 hours, Then it was cured at 200°C for 2 hours, and finally at 250°C for 2 hours to obtain a coating.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The present application provides a benzoxazine and a preparation method thereof, a coating and a method for forming a coating on the surface of a substrate. The benzoxazine is obtained by reacting curcumin, paraformaldehyde or formaldehyde, and an amine compound in an organic solvent, and then separating the reaction product; wherein, the amine compound is a compound containing a primary amine group. The coating comprises polybenzoxazine phenolic resin, and the polybenzoxazine phenolic resin is obtained by polymerizing the benzoxazine as a monomer. The benzoxazine described in the present application has excellent anti-fungal and anti-oxidation effects as well as excellent anti-corrosion, anti-adhesion and anti-fouling effects when it is suitable for forming a coating.

Description

technical field [0001] The present application relates to benzoxazines, methods for their preparation, coatings, and methods of forming coatings on substrate surfaces. Background technique [0002] Metal corrosion is very common in daily life, and its reaction process is relatively slow, but it covers almost all areas of the national economy, such as pitting and perforation of pipelines, rusting of metal components, rusting of ship hulls and bridges, etc., as long as metals are used Corrosion is a problem. The loss due to corrosion cannot be ignored. It affects the national economy, restricts the normal operation of the industry, and even causes catastrophic accidents, pollutes the environment, consumes resources, and so on. [0003] At present, researchers have explored many methods of metal anti-corrosion technology, among which, coating organic coatings on metal surfaces is a simple and effective strategy. Contents of the invention [0004] In view of the problems exi...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C07F7/18C09D161/34C09D171/02C09D5/14C09D5/08C09D5/16
CPCC07F7/1804C07F7/1892C09D161/34C09D5/14C09D5/08C09D5/1662C08L71/02
Inventor 宋光铃邓雅君郑大江
Owner XIAMEN UNIV