Preparation method of macromolecular rheological slip reducing agent
A technology of polymer and slip reducing agent, applied in the field of preparation of polymer rheological slip reducing agent, can solve the problems of odor, inconvenience and intrusion of slip reducing agent, improve working environment, improve product characteristics and improve safety Sex is also the effect of convenience
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] A preparation method of polymer rheology slip agent, the preparation method of polymer rheology slip agent comprises the following steps:
[0022] S1: Weigh or measure 100 parts of chlorosulfonated polyethylene, 5 parts of chlorinated polypropylene, 40 parts of polymer vinyl resin, 16 parts of dioctyl phthalate, and 0.06 parts of n-octadecyl propionate , 200 parts of solvent, 20 parts of lemon extract essential oil, 10 parts of peppermint leaf extract essential oil, take it for later use; the solvent in step S1 is 100 parts of xylene solvent mixed with 100 parts of ethylene glycol ether solvent;
[0023] S2: Get 100 parts of chlorosulfonated polyethylene and 5 parts of chlorinated polypropylene, add it to the inside of the stirring and heating device, open the stirring device, and stir it. In step S2, when stirring, the temperature inside the stirring device The control is 70°C, the stirring speed is set to 1200r / min, and the stirring time is 2 hours;
[0024] S3: wait...
Embodiment 2
[0029] A preparation method of polymer rheology slip agent, the preparation method of polymer rheology slip agent comprises the following steps:
[0030] S1: Weigh or measure 120 parts of chlorosulfonated polyethylene, 10 parts of chlorinated polypropylene, 45 parts of polymer vinyl resin, 20 parts of dioctyl phthalate, and 0.1 part of n-octadecyl propionate , 300 parts of solvents, 30 parts of lemon extract essential oils, 20 parts of mint leaves extract essential oils, take them for later use; the solvent in step S1 is 150 parts of xylene solvents mixed with 150 parts of ethylene glycol ether solvents;
[0031] S2: Get 120 parts of chlorosulfonated polyethylene and 10 parts of chlorinated polypropylene, add it to the inside of the stirring and heating device, open the stirring device, and stir it. In step S2, when stirring, the temperature inside the stirring device The control is 70°C, the stirring speed is set to 1200r / min, and the stirring time is 2 hours;
[0032] S3: W...
Embodiment 3
[0037] A preparation method of polymer rheology slip agent, the preparation method of polymer rheology slip agent comprises the following steps:
[0038] S1: Weigh or measure 105 parts of chlorosulfonated polyethylene, 10 parts of chlorinated polypropylene, 42 parts of polymer vinyl resin, 20 parts of dioctyl phthalate, and 0.1 part of n-octadecanyl propionate , 300 parts of solvents, 30 parts of lemon extract essential oils, 20 parts of mint leaves extract essential oils, take them for later use; the solvent in step S1 is 150 parts of xylene solvents mixed with 150 parts of ethylene glycol ether solvents;
[0039] S2: Get 105 parts of chlorosulfonated polyethylene and 10 parts of chlorinated polypropylene, add it to the inside of the stirring and heating device, open the stirring device, and stir it. In step S2, when stirring, the temperature inside the stirring device The control is 70°C, the stirring speed is set to 1200r / min, and the stirring time is 2 hours;
[0040]S3: ...