A manufacturing method and technology of plywood, applied in the direction of manufacturing tools, joining of wooden veneers, wood processing appliances, etc., can solve the problems of low production efficiency, poor quality of plywood, uneven heating, etc., and achieve high production efficiency and good product quality Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] Follow the steps below to make zero-formaldehyde plywood:
[0018] (1) Arrangement of boards: Take the rectangular aluminum plate as the reference, align the veneer and the formaldehyde-free adhesive film in sequence and fix them together by U-shaped nails. The veneer and the formaldehyde-free adhesive film form a splint, the splint and the splint Separate with rectangular pallets to form a plate group;
[0019] (2) Hot pressing: preheat the hot press to 200℃, put the plate group into the hot press for pre-pressing, the pre-pressing pressure is 3 Pa, and the pre-pressing time is 20 minutes. After the pre-pressing is completed, the hot press is Pressurize, the pressure during pressurization is 15 Pa, and the pressurization time is 10 minutes. After the pressurization is completed, the pressure is decompressed;
[0020] (3) Cold pressing: After decompression is completed, the temperature of the plate group is kept at 180°C, and the plate group is put into a cold press for press...
Embodiment 2
[0023] Follow the steps below to make zero-formaldehyde plywood:
[0024] (1) Arrangement of boards: Take the rectangular aluminum plate as the reference, align the veneer and the formaldehyde-free adhesive film in sequence and fix them together by U-shaped nails. The veneer and the formaldehyde-free adhesive film form a splint, the splint and the splint Separate with rectangular pallets to form a plate group;
[0025] (2) Hot pressing: preheat the hot press to 210°C, put the plate group into the hot press for pre-pressing, the pre-pressing pressure is 4 Pa, and the pre-pressing time is 15 minutes. After the pre-pressing is completed, the hot press Pressurize, the pressure during pressurization is 20 Pa, and the pressurization time is 9 minutes. After the pressurization is completed, the pressure is decompressed;
[0026] (3) Cold pressing: After the decompression is completed, the temperature of the plate assembly is maintained at 200°C, and the plate assembly is placed in a cold p...
Embodiment 3
[0029] Follow the steps below to make zero-formaldehyde plywood:
[0030] (1) Arrangement of boards: Take the rectangular aluminum plate as the reference, align the veneer and the formaldehyde-free adhesive film in sequence and fix them together by U-shaped nails. The veneer and the formaldehyde-free adhesive film form a splint, the splint and the splint Separate with rectangular pallets to form a plate group;
[0031] (2) Hot pressing: preheat the hot press to 220℃, put the plate group into the hot press for pre-pressing, the pre-pressing pressure is 5 Pa, and the pre-pressing time is 10 minutes. After the pre-pressing is completed, the hot press is Pressurize, the pressure during pressurization is 24 Pa, and the pressurization time is 8.5 minutes. After pressurization is completed, decompression;
[0032] (3) Cold pressing: After decompression is completed, the temperature of the plate assembly is maintained at 210°C, and the plate assembly is placed in a cold press for pressure c...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com