Secondary Li-Mn soft-packed battery and preparation method thereof
A soft packaging battery, lithium manganese technology, applied in secondary batteries, battery electrodes, battery pack components, etc., can solve the problems of poor high current output performance, difficult and flexible design of external dimensions, affecting battery charge-discharge cycle performance, etc. The effect of low cost, excellent charge-discharge and cycle performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0033] The preparation method of the secondary lithium manganese flexible packaging battery is as follows:
[0034] a. Preparation of lithium manganese composite oxide Li X MnO 2 , where 0.2≤X≤0.5;
[0035] Preparation of lithium manganese composite oxide Li 0.2~0.5 MnO 2 The specific process is: the LiNO 3 Add electrolytic manganese dioxide into a ball mill, mix evenly, and then place in a muffle furnace for 2-6 hours at 240-280°C, preferably at 260°C for 4 hours, at 320-370°C for 12-17 hours, preferably at 350°C for 15 hours, Obtain lithium manganese composite oxide Li 0.2~0.5 MnO 2 ;
[0036] b. Preparation of positive electrode
[0037] Mix and dissolve the lithium-manganese composite oxide, conductive agent, binder and pure water, stir evenly and roll it into a film on a double-roller machine. After drying, press the film and aluminum mesh to form and dry;
[0038] Among them, the mass percentage of lithium manganese composite oxide, conductive agent and binder i...
Embodiment 1
[0045] Lithium-manganese composite oxide (Li 0.2 MnO 2 ): Conductive agent: adhesive = 80:10:10 ratio of ingredients, add an appropriate amount of pure water, stir evenly, roll on a double-roller machine to form a film, after drying, press the film and aluminum mesh to form, cut The positive and negative electrodes are separated by a diaphragm, and the diaphragm is rolled into a square together with the positive and negative electrodes. After the roll is finished, the winding core is wrapped with tape to form a wound-type battery; In the membrane shell, sealing, injection of electrolyte, aging and secondary sealing molding.
Embodiment 2
[0047] Lithium-manganese composite oxide (Li 0.2 MnO 2 ): Conductive agent: adhesive = 88:7:5 ratio of ingredients, add an appropriate amount of pure water, stir evenly, roll into a film on a double-roller machine, after drying, press the film and aluminum mesh to form, cut The positive and negative electrodes are separated by a diaphragm, and the diaphragm is rolled into a square together with the positive and negative electrodes. After the roll is finished, the winding core is wrapped with tape to form a wound-type battery; In the membrane shell, sealing, injection of electrolyte, aging and secondary sealing molding.