A heat-dissipating, adapter technology, applied in the direction of connection, contact parts, contact parts manufacturing, etc., can solve the problems of short service life and poor heat dissipation effect, and achieve the effect of improving cutting performance, reducing cutting resistance and prolonging service life.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040] The composition and mass percentage ratio of contact piece brass are as follows: Cu: 59.0%, Al: 0.5%, Si: 2.5%, Sn: 0.80%, Bi: 0.6%, In: 2.0%, Fe: 0.25%, P: 0.1%, Pb ≤ 0.05%, the balance is Zn, heat the raw materials with good ratio to 1120-1180°C for melting, and fully stir;
[0041] Transfer the stirred solution into a holding furnace for horizontal continuous casting to form a semi-finished contact sheet, and then stretch, peel, and anneal to obtain a contact sheet. The temperature of the holding furnace is 700°C, and the horizontal continuous casting speed is 90mm / min. The annealing temperature is 580°C.
Embodiment 2
[0043] The composition and mass percentage ratio of contact piece brass are as follows: Cu: 62.0%, Al: 0.2%, Si: 2.5%, Sn: 0.15%, Bi: 0.8%, In: 2.0%, Fe: 0.05%, P: 0.5%, Pb ≤ 0.05%, the balance is Zn, heat the raw materials with a good ratio to 1120-1180°C for melting, and fully stir;
[0044] The stirred solution is transferred to a holding furnace for horizontal continuous casting to form a semi-finished contact sheet, and then stretched, peeled, and annealed to obtain a contact sheet. The temperature of the holding furnace is 780°C, and the horizontal continuous casting speed is 100mm / min. The annealing temperature is 620°C.
Embodiment 3
[0046] The composition and mass percentage ratio of contact piece brass are as follows: Cu: 60.0%, Al: 0.3%, Si: 1.5%, Sn: 0.22%, Bi: 0.7%, In: 0.5%, Fe: 0.15%, P: 0.3%, Pb ≤ 0.05%, the balance is Zn, heat the raw materials with good ratio to 1120-1180°C for melting, and fully stir;
[0047] Transfer the stirred solution into a holding furnace for horizontal continuous casting to form semi-finished contact pieces, and then perform stretching, peeling, and annealing to obtain contact pieces. The temperature of the holding furnace is 750°C, and the horizontal continuous casting speed is 80mm / min. The annealing temperature is 600°C.
[0048] The contact sheet made in the embodiment 1-3 of the present invention has excellent comprehensive properties, especially has higher hardness, better corrosion resistance, and then prolongs the service life of the contact sheet. The obtained contact sheet is applied to the heat-dissipating adapter, which further improves the service life of t...