A kind of antistatic EVA sole and preparation method thereof
An antistatic and antistatic agent technology, applied in the field of organic polymer compounds, can solve the problems of weakening the mechanical properties of matrix materials, failing to meet color requirements, and poor dispersion, so as to improve visual aesthetics, reduce visual aesthetic fatigue, Feel good effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0044] In the present embodiment, the antistatic EVA sole is made up of following components by weight:
[0045] EVA 5110 25 parts
[0046] EVA 7470 35 parts
[0047] Thermoplastic Elastomer 1175 16 parts
[0048] Polyamide copolymer 15 parts
[0049] Foaming agent AC 2.5 parts
[0050] Microcapsule foaming agent 2.5 parts
[0051] Cross-linking agent DCP 1.6 - 1.7 parts
[0052] Polyether-polyamide copolymer antistatic agent 4 parts
[0053] Ionomer antistatic agent 3 parts
[0054] Nano Zinc Oxide 1.8 parts
[0055] Zinc stearate 2.0 parts
[0056] Stearic acid 1.3 parts
[0057] Anti-wear agent NM-2 1.6 parts
[0058] Talcum powder 4 parts.
[0059] Step 1: Mix other raw materials except the cross-linking agent and foaming agent for banburying, adjust the banburying temperature to 100°C, keep it for 5 minutes, then add the cross-linking agent and foaming agent, and continue banburying to raise the temperature. The discharge temperature is 110°C, and after the ba...
Embodiment 2
[0063] In the present embodiment, a kind of preparation method of antistatic EVA sole is identical with the preparation method in embodiment 1, difference is:
[0064] 45 parts of EVA 5110, 15 parts of EVA 7470, 20 parts of thermoplastic elastomer 1175, 5 parts of polyether-polyamide copolymer antistatic agent, 5 parts of ionomer antistatic agent, and 1 part of wear-resistant agent NM-2;
[0065] The banburying temperature in step 1 is 98 degrees, and the discharge temperature is 108 degrees.
[0066] The antistatic EVA sole that above-mentioned preparation obtains, density 0.24g / cm 3 , Shore hardness 56, DIN wear resistance 145 mm 3, dimensional shrinkage 1.1%, rebound rate 56%, tensile strength 3.4MPa, elongation 379%, 180 degree tear strength 8.0N / mm, dynamic anti-slip coefficient smooth dry 0.59 wet 0.45, static anti-slip coefficient dry 0.57 wet 0.41, resistivity 0.14MΩ.
Embodiment 3
[0068] In the present embodiment, a kind of preparation method of antistatic EVA sole is identical with the preparation method in embodiment 1, difference is:
[0069] EVA E153F 35 parts, EVA E265F 25 parts, polyamide copolymer 10 parts, foaming agent AC 3 parts, microcapsule foaming agent 3 parts, crosslinking agent BIBP 1.7 parts, polyether-polyamide copolymer antistatic agent 2 1 part, 8 parts of ionomer antistatic agent, 1 part of anti-wear agent FY-5082E.
[0070] The antistatic EVA sole that above-mentioned preparation obtains, density 0.21g / cm 3 , Shore hardness 59, DIN wear resistance 253 mm 3 , dimensional shrinkage 1.0%, rebound rate 52%, tensile strength 3.6MPa, elongation 381%, 180 degree tear strength 5.8N / mm, dynamic anti-slip coefficient smooth dry type 0.58 wet type 0.49, static anti-slip coefficient dry type 0.53 wet 0.44, resistivity 0.63MΩ.
PUM
Property | Measurement | Unit |
---|---|---|
melting point | aaaaa | aaaaa |
density | aaaaa | aaaaa |
tensile strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology