Digital printing pretreatment sizing agent suitable for fine spinning of wool fabrics and preparation method thereof
A technology of digital printing and wool fabric, applied in the textile field, can solve the problems of unsuitable pre-treatment slurry, etc., achieve bright colors, meet visual needs, and have firm coloring effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] Get each raw material by following parts by weight:
[0033] Urea: 1 part, ammonium sulfate: 5.5 parts, AR: 1.5 parts, AP: 1.5 parts, UNI: 1 part, guar gum: 2 parts, water: 77.5 parts; AR, AP, and UNI are all purchased from Hunts, USA Man Company (the following additives related to the above are all purchased from this company);
[0034] S1: Take the guar gum, add water to dilute the guar gum by 10% by weight, stir evenly, place it for 24 hours, and set aside;
[0035] S2: Take 46.5 parts of water, 11 parts of urea, and 5.5 parts of ammonium sulfate and stir to dissolve; add 1.5 parts of AP while stirring, and then add 1.5 parts of AR, 1 part of UNI and the remaining 31 parts of water one by one after stirring evenly, and finally Add the guar gum solution diluted in S1, stir and mix evenly to obtain a slurry.
[0036] The steps of the digital printing process adopt conventional methods.
[0037] Comparative examples 1-3 are other slurry formulations in the usual test...
Embodiment 2
[0054] Get each raw material by following parts by weight:
[0055] Urea: 10, ammonium sulfate: 4, AR: 1 part, AP: 1 part, UNI: 0.5 part, guar gum: 1 part, water: 70 parts;
[0056] S1: Take the guar gum, add water to dilute the guar gum by 9% by weight, stir evenly, place it for 24 hours, and set aside;
[0057] S2: Take 42 parts of water, 10 parts of urea, and 4 parts of ammonium sulfate and stir to dissolve; add 1 part of AP while stirring, and then add 1 part of AR, 0.5 part of UNI and the remaining 28 parts of water one by one after stirring evenly, and finally Add the guar gum solution diluted in S1, stir and mix evenly to obtain a slurry.
Embodiment 3
[0059] Get each raw material by following parts by weight:
[0060] Urea: 12 parts, ammonium sulfate: 7 parts, AR: 3 parts, AP: 3 parts, UNI: 2 parts, guar gum: 3 parts, water: 80 parts;
[0061] S1: Take the guar gum, add water to dilute the guar gum by 11% by weight, stir evenly, place it for 24 hours, and set aside;
[0062] S2: Take 48 parts of water, 12 parts of urea, and 7 parts of ammonium sulfate and stir to dissolve; add 3 parts of AP while stirring, and then add 3 parts of AR, 2 parts of UNI and the remaining 32 parts of water one by one after stirring evenly, and finally Add the guar gum solution diluted in S1, stir and mix evenly to obtain a slurry.