Chlorinated rubber waterproof coating formula and preparation method thereof
A technology of chlorinated rubber and waterproof coatings, which is applied in the direction of rubber derivative coatings, wax coatings, coatings, etc., can solve the problems of complex production process difficulty, unreasonable coating formula, and high production contractors, and achieve a wide range of applications and low production costs. Low, the effect of improving waterproof performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] The invention provides a technical solution: a chlorinated rubber waterproof coating formula and preparation method thereof, comprising the following components by weight: 45 parts of film-forming substances, 58 parts of solvent, and 34 parts of emulsifier
[0018] Among them, the film-forming material includes the following components by weight: 8 parts of chlorinated rubber, 3 parts of rubber powder, 4 parts of acrylic resin, 4 parts of silicon dioxide, 3 parts of polyvinyl chloride, 3 parts of mica stone powder, 3 parts of paraffin, calcium sulfate 2 parts of powder, 3 parts of alumina, 2 parts of titanium dioxide;
[0019] The solvent comprises the following components by weight: 14 parts of water, 13 parts of ethyl acetate, 14 parts of ethylene glycol ether acetate;
[0020] The emulsifier includes the following components by weight: 18 parts of benzylphenol polyoxyethylene ether, and 11 parts of polyacrylamide.
[0021] A preparation method for chlorinated rubber...
Embodiment 2
[0029] The invention provides a technical solution: a chlorinated rubber waterproof coating formula and its preparation method, comprising the following components by weight: 85 parts of film-forming substances, 85 parts of solvent, and 54 parts of emulsifier
[0030] Among them, the film-forming material includes the following components by weight: 11 parts of chlorinated rubber, 6 parts of rubber powder, 13 parts of acrylic resin, 6 parts of silicon dioxide, 7 parts of polyvinyl chloride, 22 parts of mica stone powder, 8 parts of paraffin, calcium sulfate 7 parts of powder, 5 parts of alumina, 10 parts of titanium dioxide;
[0031] The solvent comprises the following components by weight: 28 parts of water, 25 parts of ethyl acetate, 19 parts of ethylene glycol ether acetate;
[0032] The emulsifier includes the following components by weight: 21 parts of benzylphenol polyoxyethylene ether and 19 parts of polyacrylamide.
[0033] A preparation method for chlorinated rubber ...