Elastic yarn and dyeing method thereof
A dyeing method and elastic yarn technology, applied in the field of yarn processing, can solve problems such as long production process, ineffective monitoring of density, unsatisfactory quality problems, etc., achieve short production cycle, improve winding efficiency, and good color reproduction sexual effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0048] In this embodiment, a method for dyeing elastic yarns, CF50s / 1+XLA 42D elastic yarns are selected and dyed in a dye vat with a diameter of 1400mm. The specific steps of the dyeing method are as follows:
[0049] Step 1) the loose tube process prepares a plastic non-porous bobbin (loose tube) whose outer diameter is 120mm;
[0050] Step 2) Loose tube process Wrap a transfer layer of polyester material on a 120mm plastic non-porous bobbin (in the shape of a tube with two ends open);
[0051] Step 3) Elastic yarn is loosened on the machine table of the plastic non-porous bobbin of 120mm with the outer diameter of the transfer layer;
[0052] Step 4) After the weight of the loose tube reaches 0.6kg, the machine stops loosening the tube, and the density of the loose tube is 0.28g / cm 3 ;
[0053] Step 5) Manually turn the transfer layer on the plastic non-porous bobbin from inside to outside, and wrap the elastic yarn of the outer layer; then manually transfer the elastic ...
Embodiment 2
[0062] The dyeing method of a kind of elastic yarn of present embodiment, the raw material that adopts and dyeing method are similar to embodiment 1, and main difference is:
[0063] Step 4) The density of the loose tube after the middle loose tube is 0.2g / cm 3 ;
[0064] Density after transfer in step 5) is 0.13g / cm 3 ;
[0065] Step 8) Dyeing: add water, dyes and sodium sulfate, keep warm at 50°C for 1min, then raise the temperature to 70°C at a heating rate of 1°C / min, keep warm for 30min, then add soda ash, keep warm for 40min and then drain.
Embodiment 3
[0067] The dyeing method of a kind of elastic yarn of present embodiment, the raw material that adopts and dyeing method are similar to embodiment 1, and main difference is:
[0068] Step 4) The density of the loose tube after the middle loose tube is 0.4g / cm 3 ;
[0069] Density after transfer in step 5) is 0.26g / cm 3 ;
[0070] Step 8) Dyeing: add water, dyes and sodium sulfate, keep warm at 45°C for 30 minutes, then raise the temperature to 85°C at a heating rate of 0.5°C / min, keep warm for 5 minutes, then add soda ash, keep warm for 20 minutes, and drain.
PUM
| Property | Measurement | Unit |
|---|---|---|