A tungsten disulfide lubricating oil, tungsten disulfide technology, applied in the field of lubricating oil, can solve the problem of slow reaction between tungsten and liquid sulfur, and achieve the effect of uncomplicated and stable process, good compatibility and narrow particle size distribution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0050] The invention provides a modified nano-tungsten disulfide lubricating oil additive. The components and mass fraction ratios of the modified nano-tungsten disulfide lubricating oil additive are: modified nano-tungsten disulfide accounts for 3-7%, and other additives And base oil accounts for 93-97%. The final particle size distribution of the product of the present invention is narrow, which overcomes the problem of settling in lubricating oil. The process is not complicated, stable and easy to operate, and can realize stable industrial production.
[0051] Wherein, the raw material composition of described modified nano tungsten disulfide includes:
[0052] Raw material 1: sodium sulfide, deionized aqueous solution, the mass fraction ratio is 1:2.8;
[0053] Raw material 2: tungsten hexachloride powder, its mass fraction ratio to sodium sulfide is 1:1.69
[0054] Raw material 3: silane coupling agent, accounting for 3.5% of the total amount of raw materials;
[0055] ...
Embodiment 2
[0071] A preparation method of a modified nano-tungsten disulfide lubricating oil additive, which comprises the following process steps:
[0072] (1) Preparation of modified nano-tungsten disulfide
[0073] a. Add raw material 1: filtered sodium sulfide deionized water solution into the thermal reaction kettle, then turn on the stirring, raise the temperature to 65-70°C, then add raw material 2 tungsten hexachloride powder into the thermal reaction kettle, and then Add raw material 3 silane coupling agent accounting for 3.5% of the total raw material, and carry out reaction and aging for 2 hours.
[0074] b. After 2 hours, add raw material 4 and carry out a constant temperature reaction for 30 minutes. Dark flocs begin to appear floating on the liquid surface. After 30 minutes, remove the flocs and put them into a cleaning tank, and use deionized water to repeat the process. Wash 2-3 times, form a paste, and control the surface water.
[0075] (2) Preparation of modified nan...