A kind of production process of anti-wrinkle hot water bag leather
A production process, hot water bag technology, applied in the field of PVC leather processing, can solve the problems affecting the appearance and use effect, hot water bag wrinkles, edge warping and delamination, etc., to achieve the effect of ensuring the shape and bonding effect of the base fabric
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] A production process of anti-wrinkle hot water bag leather, comprising the following steps:
[0031] (a) The base fabric is opened and shaped, and the base fabric is twill satin; the coiling tension of the base fabric is set at 1.125N to keep the base fabric loose and prevent wrinkling; the temperature is 180°C, and the speed is 7m / min; The track of the cloth opening and shaping oven adopts a parallel type, which reduces the tension of the cloth and reduces the deformation of the cloth;
[0032] (b) Paste on the base cloth, the temperature is 180°C, and the speed is 7m / min; the paste is a PU two-component paste, and it is evenly pasted on the base cloth for 2 times, and the amount of paste is 40g / m.2 times;
[0033] (c) Preparing PVC leather, laminating it with the base fabric, and adopting calendering, including (1) internal mixing, (2) open refining, (3) extrusion, (4) calendering and (5) foam embossing; PVC leather The ratio of raw materials by weight is: 45 parts o...
Embodiment 2
[0036] A production process of anti-wrinkle hot water bag leather, comprising the following steps:
[0037] (a) The base fabric is opened and shaped, and the base fabric is a long-pile fabric; the winding tension of the base fabric is 1.125N to keep the base fabric loose and prevent wrinkling; the temperature is 175°C, and the speed is 5m / min; The track of the shaping oven adopts a parallel type, which reduces the tension of the cloth and reduces the deformation of the cloth;
[0038] (b) Paste on the base cloth, the temperature is 175°C, and the speed is 5m / min; the paste is a PU two-component paste, which is evenly pasted on the base cloth twice, and the amount of paste is 35g / m.2 times;
[0039] (c) Preparing PVC leather, laminating it with the base fabric, and adopting calendering, including (1) internal mixing, (2) open refining, (3) extrusion, (4) calendering and (5) foam embossing; PVC leather The ratio of raw materials by weight is: 45 parts of PVC resin, 30.6 parts o...
Embodiment 3
[0042] A production process of anti-wrinkle hot water bag leather, comprising the following steps:
[0043] (a) The base fabric is opened and shaped, and the base fabric is short flannelette; the winding tension of the base fabric is 1.125N to keep the base fabric loose and prevent wrinkling; the temperature is 185°C, and the speed is 9m / min; The track of the shaping oven adopts a parallel type, which reduces the tension of the cloth and reduces the deformation of the cloth;
[0044] (b) Paste on the base cloth, the temperature is 185°C, and the speed is 9m / min; the paste is a PU two-component paste, and it is evenly pasted on the base cloth for 2 times, and the amount of paste is 45g / m.2 times;
[0045] (c) Preparing PVC leather, laminating it with the base fabric, and adopting calendering, including (1) internal mixing, (2) open refining, (3) extrusion, (4) calendering and (5) foam embossing; PVC leather The ratio of raw materials by weight is: 45 parts of PVC resin, 30.6 p...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology