Dyeing technology of memory type fabric
A memory and fabric technology, which is applied in the dyeing process of memory fabrics, can solve the problems of memory fabrics such as hard texture, not very smooth surface, poor elasticity, etc., to achieve consolidating shrinkage, improving color fastness, and improving The effect of the overall feel
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Example 1. The dyeing process of memory type fabric, the dyeing process of memory type fabric, is characterized in that, comprises the following steps:
[0024] A, the memory type warp-knitted gray cloth is washed to obtain the A product;
[0025] B. Carry out alkaline treatment to product A to obtain product B;
[0026] C. Pre-designate product B to obtain product C;
[0027] D, product C is put into the dyeing vat for dyeing treatment, and product D is obtained;
[0028] E. Perform reduction treatment on product D to obtain product E;
[0029] F. Finishing and finalizing product E to obtain the finished product;
[0030] The specific steps of step B are as follows: use liquid caustic soda to carry out alkaline treatment on product A, the temperature during alkaline treatment is 100-110°C, and the time is 18-22min;
[0031] The dosage ratio between liquid caustic soda and product A is 1:55-1:65.
[0032] The memory-type warp-knitted gray cloth is warp-knitted wit...
Embodiment 2
[0043] Example 2. The dyeing process of memory type fabric, the dyeing process of memory type fabric, is characterized in that, comprises the following steps:
[0044] A, the memory type warp-knitted gray cloth is washed to obtain the A product;
[0045] B. Carry out alkaline treatment to product A to obtain product B;
[0046] C. Pre-designate product B to obtain product C;
[0047] D, product C is put into the dyeing vat for dyeing treatment, and product D is obtained;
[0048] E. Perform reduction treatment on product D to obtain product E;
[0049] F. Finishing and finalizing product E to obtain the finished product;
[0050] The specific steps of step B are as follows: use liquid caustic soda to carry out alkaline treatment on product A, the temperature during alkaline treatment is 105 ° C, and the time is 20 minutes;
[0051] The dosage ratio between liquid caustic soda and product A is 1:60.
[0052] The memory-type warp-knitted gray cloth is warp-knitted with com...