Permeable ceramic brick and its production process
A permeable brick and ceramic technology, applied in the field of ceramic floor tiles, can solve problems such as inability to drain, block drainage ditch, and water accumulation in low-lying places, and achieve the effect of improving water permeability and breathability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] A ceramic permeable brick, made of waste wall and floor brick grains, feldspar powder, cellulose, and wood chips as raw materials, and sintered according to the following formula;
[0021] Formula (by weight percentage):
[0022] Waste wall and floor tiles 70
[0023] Feldspar powder 20
[0024] Cellulose 5
[0025] Sawdust 5
[0026] Appropriate amount of water
[0027] The method for producing ceramic permeable bricks is carried out in the following steps:
[0028] ① Ingredients: crush waste wall and floor tiles and sieve 4-60 meshes; sieve wood chips 20-60 meshes; soak cellulose in 10 times the weight of water to obtain a viscosity of 400-600 degrees; crush feldspar powder and sieve 200-250 meshes According to the formula, add waste wall and floor tiles, feldspar powder, cellulose, wood chips, and then add an appropriate amount of water and stir evenly;
[0029] ② Billet making: extruded into billets according to the specified size;
[0030] ③Drying: Drying in...
Embodiment 2
[0034] Formula (by weight percentage):
[0035] Waste wall and floor tiles 80
[0036] Feldspar powder 14
[0037] Cellulose 3
[0038] sawdust 3
[0039] Appropriate amount of water
[0040] In the process steps, the calcination temperature is 1200° C., the calcination time is 120 minutes, and the rest are the same as Example 1.
Embodiment 3
[0042] Formula (by weight percentage):
[0043] Waste wall and floor tiles 90
[0044] Feldspar powder 8
[0045] Cellulose 1
[0046] sawdust 1
[0047] Appropriate amount of water
[0048] In the process steps, the calcination temperature is 1300° C., the calcination time is 100 minutes, and the rest are the same as Example 1.
PUM
Property | Measurement | Unit |
---|---|---|
bending strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com