Process for producing black core card paper
A production process and technology of black core card, applied in special paper, paper, papermaking and other directions, can solve the problems of increased cost, high cost, increased cost of playing cards, etc., and achieve the effect of smooth cards, low cost, and protection of eyesight
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0043] The manufacturing process of the present invention comprises the following processes:
[0044] (1) Production of mixed white material: DC dispersant 0.21%, sodium hexametaphosphate 0.13%, caustic soda 0.09%, antifoaming agent 0.21%, kaolin 64.47%, CMC-50: 0.52%, the rest is water, put in high speed In the dispersion tank, stir for 3-4 hours, and then go through the high-speed colloid back and forth rubber mill 10 times, and store it for later use. The quality parameters of the mixed white material are as follows, solid content: 42%; viscosity: 110MPS; pH value: 6.3.
[0045] (2) latex boiling:
[0046] A. Polyvinyl alcohol spare solution:
[0047] First add water into the reaction pot, and when the water temperature reaches 60°C, add polyvinyl alcohol so that the polyvinyl alcohol content is 8% (g / g), stir while heating in the reaction pot, the temperature reaches 100°C, Until the polyvinyl alcohol is completely dissolved, keep warm for standby (the temperature is con...
Embodiment 2-6
[0067] In the production process of the present invention, the black core slurry is made and put in raw material quantity (mass percentage) and sequence, and the temperature of preparing polyvinyl alcohol solution is as follows:
[0068]
[0069] Other process operation steps are as embodiment 1.