[0007] 1) The production method is single and the application range is narrow;
[0008] 2) The luminescent powder is made of alkaline earth aluminate luminescent material, and the material is single
[0012] CN1405106A provides a kind of photochromic luminescent glass and its production method, its main feature is that it contains 85-92% of glass frit and 8-15% of luminous substance, and its various luminescent colors are determined by the composition and proportion of luminescent substance , but due to the low content of luminescent materials, it will inevitably affect the afterglow brightness of luminescent glass, and the limitations of the method lead to great limitations in the types, artistic forms, and production processes of luminescent glass.
[0013] In the prior art, the luminescent material and the matrix glass cannot achieve the purpose of organic combination in the technical conditions such as composition ratio and sintering temperature, resulting in a single variety of luminescent glass, which cannot reflect the beauty of the glass; the luminescence caused by the high sintering temperature of the glass The brightness is low; the content of luminescent powder is limited, which affects the luminous brightness; the limitation of the process affects the use range of the matrix glass; there are few production methods, and it is impossible to realize a series of defects such as a variety of luminescent glass products.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Long persistence luminescent glass and manufacturing method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0076] Preparation of long afterglow luminescent glass powder

[0077] Mix 400g of long-lasting luminescent material 14 particle size: 10-65μm and 600g matrix glass powder 6#, particle size 60-150μm, and mix uniformly to prepare luminescent glass powder specially used for producing long-lasting luminescent glass. The glass powder is irradiated with visible light for 10 minutes, and it can emit blue light in the dark, with an afterglow of more than 10 hours.

[0078] The above process is also applicable to long afterglow luminescent materials 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 15, 16, 17, 18, 19, 20, 21, 22 , 23, 24 can produce purple, blue, blue-green, yellow-green, yellow, orange-red, white, pink and other long-lasting luminescent glass powders, which can be used as raw materials for producing long-lasting luminous glass.

[0079] The matrix glass powder formula of the above process can also be applied to 3# and 4#.

Embodiment 2

[0081] Preparation of long afterglow luminescent glass block

[0082] Put the long-lasting luminescent glass powder (400g long-lasting luminescent material 10, particle size: 10-65μm and 600g matrix glass powder 6#, particle size: 50-100μm), put it in the mold of the hydraulic press and press it into a blank with a pressure of 2.2MPa , sintered in an air atmosphere at 740°C for 30min in a heating furnace, quenched in water, crushed and sieved to obtain a long afterglow luminescence glass block (particle size 0.5-5.mm), which is used as a raw material for the production of long afterglow luminescence glass. After the glass block is irradiated with visible light for 10 minutes, it can emit yellow-green light in the dark, and the afterglow lasts for more than 10 hours.

[0083] The above process of sintering at 800°C is also applicable to long afterglow luminescent materials 1, 2, 3, 4, 5, 6, 7, 8, 9, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24.

Embodiment 3

[0085] Put the long afterglow luminous glass powder (composed of long afterglow luminescent material 4, particle size: 10-30μm, 48g and matrix glass powder 3#, particle size: 60-150μm, 72g) in the hydraulic press mold with a pressure of 3.2MPa Pressed into a blank, sintered in an air atmosphere at 850°C for 40 minutes in a heating furnace, and then cooled down to room temperature at a speed of 18°C / min with the furnace, and a long-lasting blue-green milky white long-lasting luminous glass was produced. This glass can be cut, ground, drilled and processed into any shape. The long-afterglow luminous glass emits blue-green in a dark place after being irradiated with visible light for 10 minutes, and the afterglow lasts for more than 10 hours.

[0086] The above process of sintering at 800°C is also applicable to long afterglow luminescent materials 1, 2, 3, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24 can produce purple, blue, blue-green, green, yell...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
particle diameteraaaaaaaaaa
softening pointaaaaaaaaaa
spectroscopyaaaaaaaaaa
Login to view more

Abstract

A new kind of long-afterglow phosphorescent glass is composed of 5~60 wt% long-afterglow material which particle size is 10~100 um and 40~95wt% matrix glass the softening tempereture of which is 400 DEG C ~1100 DEG C.The long-afterglow phosphorescent glass can long-afterglow phosphoresce for 4 to 12 hours in the dark after stimulating by visible light or uv,the luminescence color is yellow, yellowish green,green,blue green,orange red,red etc.The line expansion coefficient of matrix glass is (15~110)*10[-7] / DEG C and the emitting spectrum is 440~650 nm.The manufacturing method of this new long-afterglow phosphorescent glass is that making the long-afterglow material and matrix glass into phosphorescent glass powder or phosphorescent glass block firstly and then producting long-afterglow phosphorescent glass according to the conventional production technology that incorporation into silicate glass,aluminate glass,lead glass and quartz glass.

Description

technical field [0001] The invention relates to material glass, in particular to a novel long afterglow luminous glass with self-luminous function and a manufacturing method thereof. Background technique [0002] In the 1990s, two types of long-lasting luminescent materials, aluminate system and silicate system, were successively invented. These two types of long-lasting luminescent materials have greatly surpassed the traditional sulfide series luminescent materials in terms of luminous brightness, afterglow time, and chemical stability. However, traditional sulfide luminescent materials have an irreplaceable role in some fields. also play an important role. [0003] Glass plays a very important role in people's daily life, and the combination of glass and luminescent materials is a new field. As a new type of material, long afterglow luminous glass has a wide range of applications in construction, energy saving, aviation, emergency lighting,...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C03C3/074C03C3/108C03C4/12
CPCC03C3/078C03C3/108C03C3/085C03C3/083C03C3/102C03C3/087C03C3/105C03C3/093C03C4/12C03C3/06C03C3/089C03C3/076C03C3/091
Inventor 肖志国戴嘉凌罗昔贤刘丽芳刘剑雄夏威
Owner DALIAN LUMINGLIGHT SCIENCE & TECHNOLOGY CO LTD
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products