Method of providing printable decorative labels for customization of portable electronic devices
An electronic device, portable technology, applied in the field of pigmented printable decorative labels, which can solve the problem of unfitting, wrinkling, decorative labels that cannot be easily applied to multiple devices
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0102] [99] The following formulation of the vinyl halide polymer material was fed into a hopper, extrusion coated, and then calendered to produce the formed film.
[0103] Ingredients Servings
[0104] PVC(K-64) 65
[0105] PVC(K-58) 35
[0106] Ethylene, vinyl acetate, carbon monoxide terpolymer
[0107] 2
[0108] Elvaloy 742 (DuPont)
[0109] Fatty polymer plasticizer, Palamoll 652 (BASF) 30
[0110] Benzophenone UV absorber 3
[0111] Barium zinc heat stabilizer, Baerostab BZ 8780 3
[0112] Acrylic processing aid, Paraloid K125 (PMMA) 2
[0113] [100] Additional examples of vinyl halide films include the following:
Embodiment 2
[0115] [101] A membrane was prepared by adding 64 parts of Solvesso 100 to the container. With a Cowles mixer at 500 rpm, 14 parts of nitrile rubber (Nipol 1312LV) were added to the vessel. When the rubber is dissolved, 3 parts of heat stabilizer (Baerostab BZ8780) and 0.75 parts of UV absorber (Chimassorb 81) are added to the container. Next, 35 parts of plasticizer (Palamoll 656) and 100 parts of polyvinyl chloride with an intrinsic viscosity of 1.22 and a K-value of 78 were slowly added to the vessel and mixing continued for approximately 30 minutes. The temperature of the material was maintained at or below 28°C. Continue mixing until the mixture, which is now a dispersion, has a maximum PVC particle size (measured with a Hegman fineness meter) of less than 10 microns. The PVC dispersion was filtered through a 25 micron filter and 55 parts of color (Kronos 2220) was added to the container. The dispersion was stirred for 1 minute and filtered with a 10 micron filter unde...
Embodiment 3-8
[0117] [102] Following the procedure of Example 2, the table below contains the materials that were added to form the PVC dispersion.
[0118] Example 3 4 5 6 7 8
[0119] Ex2 PVC 100 100 100 100 100 100
[0120] Nitrile rubber Ex2 14.5 14 5 10 15 20
[0121] Plasticizer for Ex2 16 16 16 16 16 16
[0122] Pigment of Ex2 55 53 43.5 43.5 43.5 43.5
[0123] Heat stabilizer for Ex2 3 3 3 3 3 3
[0124] UV stabilizer for Ex2 0.75 0.75 0.75 0.75 0.75 0.75
[0125] Solvent for Ex2 63.7 53 53 53 53 53
[0126] The above PVC paste is ready for coating to form a PVC film. Two coating techniques can be used: knife on roll (KOR) and reverse roll (RR). The choice of one of these two techniques depends on film thickness, quantity, paste viscosity and film quality. The white film will be coated with a reverse roll coating system since white is produced in larger quantities. Silicone-free release paper was used as the substrate for the coating. The paste was applied to release paper...
PUM
| Property | Measurement | Unit |
|---|---|---|
| stress relaxation | aaaaa | aaaaa |
| elongation at break | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 