Pure blue gel ink and method for manufacturing same
A neutral ink, ink technology, applied in ink, household appliances, applications, etc., can solve the problems of strong corrosiveness, lack of stability, poor stability, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0055] The formula of Example 1 is as follows in Table 1:
[0056] type Dosage water Deionized water 81 grams moisturizer Xylitol 10gram Auxiliary OPE-10 type surfactant 0.5g resin R-20 type acrylic resin 0.5g Anti-corrosion and mildew-proof agent benzotriazole 0.3 g dye Acid Blue 7 3 grams thickener Xanthan Gum 0.15g
[0057] Add 81 grams of water, 10 grams of humectant, 0.5 grams of auxiliary agents, 0.5 grams of resin, 0.3 grams of antiseptic and antifungal agents, and 3 grams of dyes into the reaction kettle with paddle stirring, and stir evenly; then under low-speed stirring, Slowly add the prefabricated colloid with a thickener content of 0.15 g, and after adding, increase the rotation speed and stir evenly. Finally, the finished product is obtained by filtration and defoaming.
preparation Embodiment 2
[0082] The formula of embodiment 1 is following table 4:
[0083] type Dosage water pure water 80 grams moisturizer Diethylene glycol 10gram Auxiliary OPE-9 type surfactant 0.5g resin RX-30 type acrylic resin 1.5g Anti-corrosion and mildew-proof agent Rocima623 0.3 g dye Acid Blue 9 3 grams thickener carrageenan 0.15g
[0084] Note: The Rocima623 was purchased from Rohm and Haas Company
[0085] Add 80 grams of water, 10 grams of humectant, 0.5 grams of auxiliary agents, 1.5 grams of resin, 0.3 grams of antiseptic and antifungal agents, and 3 grams of dyes into the reaction kettle with paddle stirring, and stir evenly; then under low-speed stirring, Slowly add the prefabricated colloid with a thickener content of 0.15 g, and after adding, increase the rotation speed and stir evenly. Finally, the finished product is obtained by filtration and defoaming.
[0086] The obtained product has good writ...
preparation Embodiment 3
[0088] The formula of embodiment 1 is following table 5:
[0089] type Dosage water pure water 81.5 grams moisturizer Propylene Glycol 10gram Auxiliary OPE-12 type surfactant 0.5g resin Type 4003 Acrylic Resin 2.5 grams Anti-corrosion and mildew-proof agent Kathon LXE 0.3 g dye Direct Blue 199 3 grams
[0090] thickener Hydroxyethyl cellulose 0.15g
[0091] Note: Kathon LXE was purchased from Rohm and Haas Company
[0092] Add 81.5 grams of water, 10 grams of humectant, 0.5 grams of additives, 2.5 grams of resin, 0.3 grams of antiseptic and antifungal agent, and 3 grams of dyes into the reaction kettle with paddle stirring, and stir evenly; then under low-speed stirring, Slowly add the prefabricated colloid with a thickener content of 0.15 g, and after adding, increase the rotation speed and stir evenly. Finally, the finished product is obtained by filtration and defoaming.
[0093] Th...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com