Embodiment 1
[0011] A method for making a small-sized rubber sheet, comprising the following steps:
[0012] 1. Make the mold frame, the size and thickness of the frame are determined according to the shape of the product to be produced;
[0013] 2. Place the rubber semi-finished product in the frame, cover the upper and lower surfaces with 0.8mm galvanized white iron skin, pass the covered frame through the vulcanizing machine, the pressure is 5MPa, the temperature is 120°C, and the time is 18 minutes;
[0014] 3. After cooling, take it out and put it in a clean storage area at room temperature.
Embodiment 2
[0016] A method for making a small-sized rubber sheet, comprising the following steps:
[0017] 1. Make the mold frame, the size and thickness of the frame are determined according to the shape of the product to be produced;
[0018] 2. Place the rubber semi-finished product in the frame, cover the upper and lower surfaces with 1.0mm cold-rolled plate, pass the covered frame through the vulcanizer, the pressure is 13MPa, the temperature is 150°C, and the time is 8 minutes;
[0019] 3. After cooling, take it out and put it in a clean storage area at room temperature.
Embodiment 3
[0021] A method for making a small-sized rubber sheet, comprising the following steps:
[0022] 1. Make the mold frame, the size and thickness of the frame are determined according to the shape of the product to be produced;
[0023] 2. Place the rubber semi-finished product in the frame, cover the upper and lower surfaces with 1.2mm cold-rolled plate, pass the covered frame through the vulcanizer, the pressure is 18MPa, the temperature is 180°C, and the time is 5 minutes;
[0024] 3. Cool down, take it out and put it in a clean storage area at room temperature.