Preparation method of rubber glove with foaming on lining
A foamed rubber and foamed rubber technology, which is applied in gloves, clothing, clothing, etc., can solve the problems of airtightness of hands, no solution to wearing comfort, and easy sweating of hands, and achieve the effect of soft and elastic texture.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] A kind of preparation of latex foam rubber material: unit (kg)
[0020] 60% latex 10
[0021] 20% KOH 0.09
[0022] 50% sulfur 0.144
[0023] 50% Accelerator ZDEC 0.096
[0024] 50% Accelerator: BZ 0.024
[0026] 50% Antioxidant L 0.18
[0027] 50% sodium silicofluoride 0.108
[0028] (1) Put the above raw materials into a foaming machine and stir at high speed for 10 minutes at a speed of 800 rpm. After foaming, adjust the speed to 150 rpm for 5 minutes of uniform foaming and set aside.
[0029] (2) Immerse the hand model dipped in latex once into the above-mentioned foamed latex for 10 seconds, then lift it up at a constant speed to even out the glue, and put it in an oven for drying after the foamed glue is slightly shaped.
[0030] (3) The finished product is obtained through conventional stripping, post-treatment chlorination, soaking cleaning, and drying processes.
[0031] The natural latex gloves made by the above method have...
Embodiment 2
[0033] A kind of preparation of nitrile foamed rubber material: unit (kg)
[0034] 43% Nitrile Latex: 10
[0035] 20% KOH 0.1075
[0036] 50% sulfur 0.172
[0037] 50% accelerator ZDEC 0.086
[0038] 50% Accelerator BZ 0.043
[0040] 50% Antioxidant L 0.129
[0041] 50% sodium silicofluoride 0.108
[0042] (1) Put the above-mentioned raw materials into a foaming machine and stir at high speed for 12 minutes at a speed of 1000 rpm. After foaming, adjust the speed to 150 rpm for 6 minutes of uniform foaming and set aside. Dip the hand mold dipped in the nitrile latex once into the above-mentioned foamed latex for 8 seconds, then lift it up at a constant speed to even out the glue. After the foamed glue is slightly shaped, put it in an oven for drying.
[0043] (2) The finished product is obtained through conventional stripping, post-treatment chlorination, soaking cleaning, and drying processes.
[0044] The nitrile rubber gloves made by the...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com