Embodiment 1
[0037] Example 1 Preparation of metal adsorbent
[0038] (1) firstly clean the raw material persimmon fruit or persimmon skin containing persimmon tannin, crush or squeeze the juice, and obtain persimmon powder containing persimmon tannin after vacuum freeze-drying at 40-200Mpa for 10-40h, and set aside;
[0039] (2) Add 0.125-0.25mol / L sodium hydroxide solution to the persimmon tannin-containing persimmon powder obtained in step 1, fully stir and mix, then add 37% formaldehyde solution by v / v, fully stir , to obtain the solid granular adsorbent crude product containing persimmon tannin;
[0040] 3) Put the crude adsorbent product obtained in step 2) in a water bath, the temperature of the water bath is 81°C, and the water bath time is 24h, so that it can fully react; the crude adsorbent product after the reaction is washed once with deionized water, and then washed with 100mL 0.05 Wash once with mol / L dilute nitric acid solution, and finally wash with deionized water repeate...
Embodiment 2
[0041] Example 2 Adsorption and recovery of precious metal gold by persimmon tannin
[0042] (1) The pH value of the mixed solution containing gold ions is adjusted to 2-4;
[0043] (2) Put the metal adsorbent into the Erlenmeyer flask, react with the mixed solution containing gold ions, and seal it with a parafilm; in mg / mL, the mass ratio of the metal adsorbent to the mixed solution containing gold ions 1:3-5, the total volume is less than 1 / 2 of the volume of the Erlenmeyer flask;
[0044](3) The mixture of the metal adsorbent that has adsorbed gold in step (2) is incinerated with a flame until the impurities in the metal adsorbent are completely burned to obtain pure gold, or eluted with 1mol / L eluent thiourea The metal adsorbent mixture that has adsorbed gold for 12-24 hours to obtain a concentrated eluent, and further remove the liquid in the eluent to obtain pure gold;
[0045] in:
[0046] The reaction conditions in the non-metal container are: vibration adsorption,...
Embodiment 3
[0047] Example 3 Adsorption and recovery of precious metal gold by persimmon tannin metal adsorbent
[0048] (1) The pH value of the mixed ion solutions (shown in Table 1) containing gold ions of different concentrations is adjusted to 2;
[0049] (2) The metal adsorbent of embodiment 1 and the gold ion mixed solution of step (1) are added in the Erlenmeyer flask by mg / mL, and the volume ratio of the metal adsorbent mass to the solution is 1: 3-5;
[0050] (3) Seal the triangular flask with a sealing film, put it into a shaker with a preset temperature of 30-50°C and a rotation speed of 100-200rpm, oscillate and adsorb for 24 hours, filter, and the gold ions can be completely adsorbed by the adsorbent;
[0051] (4) The method for further recovering pure gold in the metal adsorbent refers to step (3) of Example 1.
[0052] The initial concentrations of ions in the four adsorption systems of the present invention are shown in Table 1.
[0053] Table 1 Initial concentrations of...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com