[0042] Component mass ratio
[0043] ①Water 25
[0044] ②Surfactant 0.5
[0045] ③Anticorrosion and fungicide 0.1
[0046] ④Titanium dioxide 15
[0047] ⑤ Coalescing agent 2
[0048] ⑥ thickener solution 15
[0049] ⑦Emulsion 34.4
[0050] ⑧Light perlite 8
[0051] The preparation method of the lightweight sound-absorbing and environment-friendly interior wall coating is as follows:
[0052] Add water, surfactant, antiseptic and bactericide into the container, stir with the mixer at low speed (about 500 rpm), slowly add titanium dioxide, increase the stirring speed and disperse at high speed (about 1200 rpm) for 20-30 minutes, then adjust Lower the speed of the mixer to 300-600 rpm, gradually and slowly add film-forming aids, thickener solution, emulsion, light perlite, and disperse for 15-20 minutes.
Embodiment 2
[0054] Component mass ratio
[0055] ①Water 30
[0056] ② Surfactant 1.5
[0057] ③Anticorrosion and fungicide 0.3
[0058] ④Titanium dioxide 15
[0059] ⑤ Coalescing agent 2
[0060] ⑥ thickener solution 14.2
[0061] ⑦ Emulsion 25
[0062] ⑧Light perlite 12
[0063] The preparation method of the lightweight sound-absorbing and environment-friendly interior wall coating is as follows:
[0064] Add water, surfactant, antiseptic and bactericide into the container, stir with the mixer at low speed (about 500 rpm), slowly add titanium dioxide, increase the stirring speed and disperse at high speed (about 1200 rpm) for 20-30 minutes, then adjust Lower the speed of the mixer to 300-600 rpm, gradually and slowly add film-forming aids, thickener solution, emulsion, light perlite, and disperse for 15-20 minutes.
Embodiment 3
[0066] Component mass ratio
[0067] ① water 26
[0068] ②Surfactant 1
[0069] ③Anticorrosion and fungicide 0.2
[0070] ④Titanium dioxide 10
[0071] ⑤ Coalescing agent 5
[0072] ⑥ thickener solution 12.8
[0073] ⑦ Emulsion 34
[0074] ⑧Light perlite 11
[0075] The preparation method of the lightweight sound-absorbing and environment-friendly interior wall coating is as follows:
[0076] Add water, surfactant, antiseptic and bactericide into the container, stir with the mixer at low speed (about 500 rpm), slowly add titanium dioxide, increase the stirring speed and disperse at high speed (about 1200 rpm) for 20-30 minutes, then adjust Lower the speed of the mixer to 300-600 rpm, gradually and slowly add film-forming aids, thickener solution, emulsion, light perlite, and disperse for 15-20 minutes.
[0077] A preferred embodiment of the present invention:
[0078] Component mass ratio
[0079] ① water 28
[0080] ② Surfactant 1.2
[0081] ③Anticorrosion and fun...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
solid content | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com