[0021] The manufacturing method of fir flooring, its operation steps are as follows:
[0022] a. Saw board: saw the fir with a tail diameter of 80 mm into a board with a thickness of 22 mm;
[0023] b. Health preservation: Put the boards in a rain-proof and ventilated environment and dry them for 10 days. Use multiple 22mm×22mm wooden strips between each layer of boards for upper and lower intervals;
[0024] c. Drying: Put the finished plates in the drying cellar and dry them to the moisture content range of 8% to 13%, and then exit the cellar;
[0025] d. Shaping: stack the boards out of the kiln to dry for 6 days in a rain-proof and ventilated environment, and use multiple 22mm×22mm wooden strips between each layer of boards for upper and lower intervals;
[0026] e. Saw blade: sawing the finished plate into a square strip with a square cross-section, the side length of the square: 22 mm × 22 mm;
[0027] f. Selection: After cutting off the decayed section of the square strips, the sq...
Embodiment 2
[0033] The manufacturing method of fir flooring, its operation steps are as follows:
[0034] a. Saw board: Saw a fir with a tail diameter of 120 mm into a board with a thickness of 24 mm;
[0035] b. Health preservation: Put the boards in a rain-shielded and ventilated environment and dry them for 15 days. Use multiple 24 mm x 24 mm wooden strips between each layer of boards for upper and lower intervals;
[0036] c. Drying: Put the finished plates in the drying cellar and dry them to the moisture content range of 8% to 13%, and then exit the cellar;
[0037] d. Shaping: Stack the boards out of the kiln to dry for 8 days in a rain-shielded and ventilated environment, and use multiple 24mm×24mm wooden strips between each layer of boards for upper and lower intervals;
[0038] e. Saw blade: sawing the finished sheet into a square strip with a square cross section, the side length of the square is: 24 mm × 24 mm;
[0039] f. Selection: Use the strategy of having at least one side surface i...