Processing method of environment-friendly ternary elastic plastic floor
An elastic plastic, processing method technology, applied in the superstructure sub-assembly, transportation and packaging, superstructure and other directions, can solve the problems of poor wear resistance and slip resistance, no sound insulation and shock absorption, environmental hazards, etc., and achieve stiffness Good, low deformation rate, good thermoforming performance
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2015-08-12
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to a processing method of a plastic floor, in particular to a car floor and a processing method of the car floor. Background technique
[0002] Most of the existing car floors are PVC or HIPS plastic floors, which will emit harmful gases, which will cause harm to the human body and the environment; environmentally friendly floors will be the development trend of car floors in the future, and non-environmental-friendly floors will Gradually withdraw from the market; at the same time, the traditional car floor has poor wear resistance and skid resistance, and does not have the function of sound insulation and shock absorption, which has become one of the important sources of noise in the car. Contents of the invention
[0003] The technical problem to be solved by the present invention is to provide an environment-friendly floor processing method for the above-mentioned deficiencies in the prior art. The floor processed by this pr...
Examples
Embodiment 1
[0040] The processing method of environment-friendly ternary elastic plastic floor,
[0041] The first is the steps to make the floor ternary elastomer layer:
[0042] (1) Mix the mixture of ethylene, propylene, butene and additives at 120°C for 15 minutes at high speed and 15 minutes at low speed, wherein the speed of high speed mixing is 1000 rpm, and the speed of low speed mixing is 1000 rpm. 70 rpm;
[0043] (2) Send the mixture prepared in step (1) into a twin-screw granulator for granulation, and the temperature in the granulator is controlled at 220° C.;
[0044] (3) The granules obtained in step (2) are sent to the auxiliary machine of the extruder, extruded and shaped, the temperature in the auxiliary machine is controlled between 200 ° C, the extrusion speed is 60 rpm, and the extrusion pressure is 8kg; the floor ternary elastomer layer is obtained; in this step, the extruder includes a main engine and an auxiliary machine, and the settings of the main engine and t...