Unlock instant, AI-driven research and patent intelligence for your innovation.

A kind of antistatic plastic and preparation method thereof

A technology of antistatic plastics and parts resistance, applied in the field of antistatic plastics, can solve the problems of unstable quality of antistatic plastics, high product cost, low working temperature, etc., to avoid damage to electronic components, good antistatic performance, high gap The effect of impact strength

Active Publication Date: 2015-11-25
ANHUI ANYUAN PLASTIC
View PDF4 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, general-purpose plastics on the market have low thermal conductivity, low operating temperature, high hardness of fillers, great wear and tear on equipment, and are prone to static electricity.
[0003] The quality of the existing antistatic plastics on the market is not stable, its bending strength and hardness are not high, and its service life is short, which cannot meet the requirements of the existing market for materials; and some plastics with better effects have undergone complicated processes. Made, but the product cost is too high
For example, Chinese patent 201210311205.2 discloses a formula for antistatic plastics and a formula for antistatic modified plastics disclosed in 201210261587.2. The antistatic plastics disclosed in these two patents have low bending strength and hardness and short service life.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A kind of antistatic plastic and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0016] An antistatic plastic, which is mainly made of the following raw materials according to the ratio of parts by mass: 110-130 parts by mass of PVC, 30-35 parts by mass of PP, 30-40 parts by mass of ABS, 10-15 parts by mass of aliphatic sulfonic acid Salt, 5-8 parts by mass of tribasic lead sulfate, 4-8 parts by mass of catalyst, 5-10 parts by mass of antistatic agent, 10-20 parts by mass of carbon black, 6-10 parts by mass of hydroxymethyl fatty amine, 10- 20 parts by mass of impact modifier, 10-15 parts by mass of graphite, 3-6 parts by mass of cocatalyst, 5-10 parts by mass of dibasic lead phosphite and 1-5 parts by mass of white oil.

[0017] Another preferred solution of the present invention: an antistatic plastic, which is mainly made of the following raw materials according to the ratio of parts by mass: 110-130 parts by mass of PVC, 30-35 parts by mass of PP, 30-40 parts by mass of ABS, 10 parts by mass -15 parts by mass of aliphatic sulfonate, 5-8 parts by mass o...

Embodiment 2

[0026] An antistatic plastic, which is mainly made of the following raw materials according to the ratio of parts by mass: 110 parts by mass of PVC, 30 parts by mass of PP, 30 parts by mass of ABS, 10 parts by mass of aliphatic sulfonate, 5 parts by mass of tribasic Lead sulfate, 4 parts by mass of sodium hydroxide, 5 parts by mass of antistatic agent S-15, 10 parts by mass of carbon black with a particle size of 80-120 mesh, 16 parts by mass of hydroxymethyl aliphatic amine, 10 parts by mass of impact modifier CPE , 10 parts by mass of graphite with a particle size of 300-310 μm, 3 parts by mass of acetyl caprolactam, 5 parts by mass of dibasic lead phosphite and 1 part by mass of white oil.

[0027] The method for preparing the above-mentioned antistatic plastics comprises the following steps: firstly mix each component fully and evenly, then add them into a twin-screw extruder to melt, plasticize and granulate them at a temperature of 170°C and a screw speed of 80r / min; Inj...

Embodiment 3

[0029] An antistatic plastic, which is mainly made of the following raw materials according to the ratio of parts by mass: 120 parts by mass of PVC, 32 parts by mass of PP, 34 parts by mass of ABS, 13 parts by mass of aliphatic sulfonate, 6 parts by mass of tribasic Lead sulfate, 5 parts by mass of sodium hydroxide, 7 parts by mass of antistatic agent SN, 14 parts by mass of carbon black with a particle size of 80-120, 6 parts by mass of hydroxymethyl fatty amine, 10 parts by mass of impact modifier CPE, 10 parts by mass of Parts by mass of graphite with a particle size of 300-310 μm, 3 parts by mass of acetyl caprolactam, 5 parts by mass of dibasic lead phosphite and 1 part by mass of white oil.

[0030] The method for preparing the above-mentioned antistatic plastics comprises the following steps: firstly mix each component fully and evenly, then add them into a twin-screw extruder to melt, plasticize and granulate them at a temperature of 180°C and a screw speed of 85r / min; ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
particle sizeaaaaaaaaaa
particle diameteraaaaaaaaaa
electrical resistivityaaaaaaaaaa
Login to View More

Abstract

The invention discloses an antistatic plastic and a preparation method thereof. The antistatic plastic is mainly prepared from the following raw materials in parts by mass: 110-130 parts of PVC (polyvinyl chloride), 30-35 parts of PP (polypropylene), 30-40 parts of ABS (acrylonitrile-butadiene-styrene), 10-15 parts of fatty group sulfonate, 5-8 parts of tribasic lead sulfate, 4-8 parts of catalyst, 5-10 parts of antistatic agent, 10-20 parts of carbon black, 6-10 parts of hydroxymethyl fatty amine, 10-20 parts of shock-resistant modifier, 10-15 parts of graphite, 3-6 parts of cocatalyst, 5-10 parts of dibasic lead phosphite and 1-5 parts of white oil. The preparation method comprises the following steps: thoroughly mixing the components uniformly; adding the mixture into a double screw extruder; granulating by melting and plastification under certain conditions; and carrying out injection molding on the granules under certain conditions. The method disclosed by the invention is simple in technique, and convenient for large-scale production; and the product has the advantages of high notch impact strength, high bending strength, high hardness, and favorable antistatic property.

Description

technical field [0001] The invention belongs to the field of polymer materials, and in particular relates to an antistatic plastic. technical background [0002] Plastic material is a material with good performance. Because plastic has the advantages of light weight, no rust, and good insulation, it is used in many aspects of electronic product production. Plastic is easy to process, has good dimensional stability and surface gloss, and is easy to paint. Coloring, widely used in the field of electronic appliances. In recent years, in the electronic and electrical market, plastics have to maintain their position in the electronic and electrical market, and their performance must be improved. For example, the generation of static electricity will bring many troubles, such as electrostatic discharge, which will harm electronic equipment, cause various failures of equipment, and shorten the service life. With the expansion of the market for electronic and electrical products,...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C08L27/06C08L23/12C08L55/02C08K13/02C08K5/42C08K3/30C08K3/04C08K5/17C08K3/32C08K5/12B29B9/06B29C47/92B29C45/76B29C48/92
CPCB29C47/92B29C2947/92514B29C2947/92704B29C2947/92895B29C48/40B29C48/92B29C2948/92514B29C2948/92704B29C2948/92895
Inventor 汤毅