A technology of rock flake paint and rotating speed, which is applied to paints containing biocide, anti-fouling/underwater paints, coatings, etc., can solve the problems of paint creation and short service life, and improve stain resistance Durability and weather resistance, simple construction, and reduced maintenance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0042] A rock flake paint, comprising component A and component B, wherein the composition of component A and the mass percentage of the total mass of the rock flake paint are:
[0043] Water-based acrylic emulsion: 15%
[0044] Coalescing aids: 1.5%
[0045] Defoamer: 0.25%
[0046] Antiseptic and antifungal agent: 0.8%
[0047] Hydroxyethylcellulose: 0.15%
[0048] water 10;
[0049] The composition of component B and the mass percentage of the total mass of rock flake paint are:
[0050] Aggregate: 64%
[0051] Composite rock slice 8.3%.
[0052] A method for preparing the above rock flake paint, comprising the following steps:
[0053] (1) Preparation of component A
[0054] (a) Put water into a clean paint vat, start the disperser and stir at 200RPM;
[0055] (b) Add film-forming aids and defoamers in sequence, and disperse for 3 minutes at 200 RPM;
[0056] (c) Add cellulose ether and disperse at 200RPM for 3 minutes;
[0057] (d) When the cellulose ether is c...
Embodiment 2
[0062] A rock flake paint, comprising component A and component B, wherein the composition of component A and the mass percentage of the total mass of the rock flake paint are:
[0063]
[0064]
[0065] The composition of component B and the mass percentage of the total mass of rock flake paint are:
[0066] Granite gravel: 70%
[0067] Composite rock slice 9%.
[0068] A method for preparing the above rock flake paint, comprising the following steps:
[0069] (1) Preparation of component A
[0070] (a) Put water into a clean paint vat, start the disperser and stir at 300RPM;
[0071] (b) Add film-forming aids and defoamers in turn, and disperse for 3 minutes at 300 RPM;
[0072] (c) Add cellulose ether and disperse at 300RPM for 3 minutes;
[0073] (d) When the cellulose ether is completely wetted and stirred evenly, adjust the pH to 8.0-9.0, and when the viscosity increases, increase the speed to 2000RPM to disperse for 3 minutes;
[0074] (e) Put in the emulsio...
Embodiment 3
[0078] A rock flake paint, comprising component A and component B, wherein the composition of component A and the mass percentage of the total mass of the rock flake paint are:
[0079] Water-based acrylic emulsion: 15%
[0080] Coalescing aids: 1.5%
[0081] Defoamer: 0.25%
[0082] Antiseptic and antifungal agent: 0.8%
[0083] Hydroxyethylcellulose: 0.15%
[0084] water 10;
[0085] The composition of component B and the mass percentage of the total mass of rock flake paint are:
[0086] Aggregate: 64%
[0087] Composite rock slice 8.3%.
[0088] A method for preparing the above rock flake paint, comprising the following steps:
[0089] (1) Preparation of component A
[0090] (a) Put water into a clean paint vat, start the disperser and stir at 200RPM;
[0091] (b) Add film-forming aids and defoamers in sequence, and disperse for 3 minutes at 200 RPM;
[0092] (c) Add cellulose ether and disperse at 200RPM for 3 minutes;
[0093] (d) When the cellulose ether is com...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com