Really stone paint
A technology of real stone paint and quartz sand, applied in the field of paint manufacturing, can solve the problems of inability to "touch nature, heavy quality of natural stone, and high price of natural stone, reduce the phenomenon of sand falling, improve construction, and improve usability". Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0049] The purpose of this embodiment is to provide a real stone paint.
[0050] This embodiment specifically provides a kind of genuine stone paint, which is also composed of the following mass fraction components in addition to the pH regulator:
[0051] Water: 17.50~18.50%,
[0052] Hydroxyethyl cellulose: 0.25-0.35%,
[0053] Concentrated 168: 0.05~0.07%,
[0054] Strengthening agent: 0.05~0.07%,
[0055] Stabilizer: 0.05~0.07%,
[0056] Emulsion: 9.50~10.50%,
[0057] Film-forming aids: 0.45-0.55%,
[0058] Quartz sand: 70.00~72.00%;
[0059] The method of preparing real stone paint is: add water into the mixing tank, add hydroxyethyl cellulose, concentrate 168, strengthening agent, stabilizer, emulsion, and film-forming aid in turn under stirring, and stir evenly; then add quartz sand, Stir evenly, adjust the viscosity; adjust the pH value to 7.0-12.0 with a pH regulator, and pack after passing the inspection.
[0060] Specifically, in addition to the pH regulato...
Embodiment 2
[0092] A real stone paint, composed of the following components by mass fraction: 17.82% water, 0.30% hydroxyethyl cellulose, 0.06% concentrated 168, 0.06% strengthening agent, 0.06% stabilizer, 9.90% emulsion, 0.50% film-forming Auxiliary, 71.30% quartz sand, pH adjuster in proper amount.
[0093] In this example:
[0094] The strengthening agent is specifically a combination of defoaming agent, antiseptic, antifungal agent and antibacterial agent, and the specific ratio is 6:4:8:1.
[0095] The stabilizer is specifically a liquid stabilizer; the stabilizer can maintain the balance of chemical raw materials, reduce surface tension, prevent light and heat from decomposing and oxidizing raw materials, and ensure the stability of fibers.
[0096] The emulsion is styrene-acrylic emulsion;
[0097] The film-forming aids are propylene glycol butyl ether and propylene glycol butyl ether acetate, and the mixing ratio is 1:1;
[0098] The particle size of the quartz sand is quartz ...
Embodiment 3
[0114] A real stone paint, composed of the following components by mass fraction: 17.70% water, 0.25% hydroxyethyl cellulose, 0.05% concentrated 168, 0.07% strengthening agent, 0.05% stabilizer, 9.50% emulsion, 0.45% film-forming Appropriate amount of additives, 71.93% quartz sand, and pH regulator;
[0115] In this example:
[0116] The strengthening agent is a combination of defoaming agent, antiseptic and antifungal agent, and the specific ratio is 3:2:4.
[0117] The stabilizer is a composite stabilizer.
[0118] The emulsion is silicone acrylic emulsion.
[0119] The film-forming aid is propylene glycol butyl ether.
[0120] The particle size of the quartz sand is quartz sand within the range of 20 to 180 mesh, specifically snowflake white colored sand.
[0121] The pH regulator is boric acid and potassium dihydrogen phosphate.
[0122] The method of preparing real stone paint is:
[0123] Add water into the mixing tank, add hydroxyethyl cellulose, concentrate 168, ...
PUM
Property | Measurement | Unit |
---|---|---|
Bond strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com