Preparation method of low-smoke and non toxicity cable sheath
A cable sheath and temperature control technology, applied to plastic/resin/wax insulators, organic insulators, etc., can solve problems such as dense, odorous, flammable and toxic smoke from cable sheaths, and reduce toxic gas, reduce consumption, and suppress The effect of thermal oxidation degradation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] The preparation method of low-smoke and non-toxic cable sheath comprises the following steps:
[0027] 1) Ingredients
[0028] Take the following raw materials by weight: 40 parts of SG-2 type resin, 25 parts of diisodecyl phthalate,
[0029] 2 parts of calcium / zinc composite stabilizer and 1 part of bisphenol A, the ingredients are refined and mixed thoroughly, the fineness after refining is less than or equal to 70 μm, and the main material after refining is obtained;
[0030] 2) Add filler
[0031] Add 50 parts of calcined calcium carbonate and 0.1 part of stearic acid to the main material after refining, stir evenly and then re-refining, the fineness after refining is less than or equal to 60 μm, to obtain the main material after re-refining;
[0032] 3) Knead
[0033] Control the temperature at 50°C, and knead the main material after re-refining for 4 minutes;
[0034] 4) Extrusion
[0035] Control the temperature at 140°C and extrude;
[0036] 5) Refining
...
Embodiment 2
[0039] The preparation method of low-smoke and non-toxic cable sheath comprises the following steps:
[0040] 1) Ingredients
[0041] Take the following raw materials by weight: 50 parts of SG-2 type resin, 30 parts of diisodecyl phthalate,
[0042] 4 parts of calcium / zinc composite stabilizer and 2 parts of bisphenol A, the ingredients are refined and mixed thoroughly, the fineness after refining is less than or equal to 70 μm, and the main material after refining is obtained;
[0043] 2) Add filler
[0044] Add 60 parts of calcined ceramic clay and 1 part of stearic acid to the main material after refining, stir evenly and then refine the slurry again, and the fineness after refining is less than or equal to 60 μm to obtain the main material after re-refining;
[0045] 3) Knead
[0046] Control the temperature at 75°C, and knead the main material after re-refining for 10 minutes;
[0047] 4) Extrusion
[0048] Control the temperature at 160°C and extrude;
[0049] 5) R...
Embodiment 3
[0052] The preparation method of low-smoke and non-toxic cable sheath comprises the following steps:
[0053] 1) Ingredients
[0054] Take the following raw materials by weight: 85 parts of SG-2 type resin, 28 parts of diisononyl phthalate
[0055] 5 parts of calcium / zinc composite stabilizer and 2.5 parts of bisphenol A, the ingredients are refined and mixed thoroughly, the fineness after refining is less than or equal to 70 μm, and the main material after refining is obtained;
[0056] 2) Add filler
[0057] 40 parts of calcined ceramic clay and 20 parts of calcium carbonate were added to the main material after refining, and after stirring evenly, the slurry was re-refined, and the fineness after refining was less than or equal to 60 μm to obtain the main material after re-refining;
[0058] 3) Knead
[0059] Control the temperature at 70°C, knead the main material after re-refining for 8 minutes;
[0060] 4) Extrusion
[0061] Control the temperature at 155°C and extr...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com