Water-based environment-friendly automotive paint surface repairing wax and preparing method thereof
An environmentally friendly, automotive paint technology, applied in wax coatings, coatings, etc., can solve the problems of solvent volatile environment, short gloss and protection time, pollution, etc., achieve simple and easy preparation process steps, good removal of scratches and Filling the paint surface and expanding the effect of comprehensive performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0052] The water-based environment-friendly car paint repair wax of the present embodiment comprises the following components by weight:
[0053] 5 parts of environment-friendly aliphatic hydrocarbon solvent, 1 part of acid montan wax, 1 part of simethicone, 1 part of surfactant, 1 part of polyol, 5 parts of polishing powder, 1 part of thickener, 0.1 part of preservative, pigment 0.01 parts, 30 parts of deionized water.
[0054] The preparation method of the water-based environment-friendly car paint repair wax of the present embodiment may further comprise the steps:
[0055] (1) Weigh in order according to parts by weight and put 5 parts of aliphatic hydrocarbon solvent, 1 part of acid montan wax, and 1 part of simethicone oil into the oil pan, and heat up to 80 ° C under the condition of constant stirring. Dissolve completely in the form of a transparent liquid, keep the temperature for 5 minutes;
[0056] (2) Add 30 parts of deionized water, 1 part of surfactant, 1 part ...
Embodiment 2
[0059] The water-based environment-friendly car paint repair wax of the present embodiment comprises the following components by weight:
[0060] 20 parts of environment-friendly aliphatic hydrocarbon solvent, 10 parts of acid montan wax, 10 parts of simethicone, 5 parts of surfactant, 5 parts of polyol, 20 parts of polishing powder, 5 parts of thickener, 1 part of preservative, pigment 0.1 part, 70 parts of deionized water.
[0061] The preparation method of the water-based environment-friendly car paint repair wax of the present embodiment may further comprise the steps:
[0062] (1) Weigh and put 20 parts of aliphatic hydrocarbon solvent, 10 parts of acid montan wax, and 10 parts of simethicone oil into the oil pan in order by weight parts, and heat up to 95 ° C under the condition of constant stirring. Dissolve completely in the form of a transparent liquid, keep the temperature for 30 minutes;
[0063] (2) Add 70 parts of deionized water, 5 parts of surfactant, 5 parts ...
Embodiment 3
[0066] The water-based environment-friendly car paint repair wax of the present embodiment comprises the following components by weight:
[0067] 15 parts of environment-friendly aliphatic hydrocarbon solvent, 5 parts of acid montan wax, 5 parts of dimethyl silicone oil, 3 parts of surfactant, 3 parts of polyol, 15 parts of polishing powder, 3 parts of thickener, 0.5 part of preservative, pigment 0.05 parts, 50 parts of deionized water.
[0068] The preparation method of the water-based environment-friendly car paint repair wax of the present embodiment may further comprise the steps:
[0069](1) Weigh and put 15 parts of aliphatic hydrocarbon solvent, 5 parts of acid montan wax, and 5 parts of simethicone oil into the oil pan in order by weight parts, and heat up to 90 ° C under the condition of constant stirring. Dissolve completely in the form of a transparent liquid, keep the temperature for 15 minutes;
[0070] (2) Add 50 parts of deionized water, 3 parts of surfactant,...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap